Transcript
Page 1: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

Welding procedures and welders

Guidelines on approval testingWG 01

Page 2: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

© 2012 Safety Assessment Federation (SAFed)

The Safety Assessment Federation SAFed represents the interests of companies engaged in independent inspection and safety assessment of engineering and

manufacturing plant, systems and machinery.

Proposed revisions should be notified to the SAFed technical manager.

Issue Date Pages

01 1998 New document

02 November 2012 New document

ISSUE STATUS AND REVISIONS

Page 3: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

3 of 55

The mechanical integrity of plant containing hazardous substances

A guide to periodic examination and testing

Edition 1 - September 2012

Table of Contents: Page

CONTENTS

1 INTRODUCTION 4

2 OBTAINING WELDING CERTIFICATION 5

3 WELDING OF TESTPIECES 7

4 TESTING 8

5 CERTIFICATION 9

6 SAFed MEMBER COMPANY SERVICES 10

APPENDIX I 11

WELDING PROCEDURE APPROVAL TEST CERTIFICATE E1 12

DETAILS OF WELD CERTIFICATE E2 13

DETAILS OF WELD CERTIFICATE E2 (CONTINUATION SHEET) 14

TEST RESULTS CERTIFICATE E3 15

WELDER APPROVAL TEST CERTIFICATE E4 16

APPENDIX 11 17

Welding procedures and welders

Guidelines on approval testing

Page 4: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

4 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

1.0 INTRODUCTION

1.1 Welding approvals

The practice of approval testing of welding procedures and welders has been employed for

over half a century. Approval testing is carried out prior to production commencing and it

is therefore essentially a quality assurance measure rather than a quality control activity.

1.2 Commonly used terms

The more commonly used terms associated with welding approvals are as follows:

• Preliminary Welding Procedure Specification (pWPS)This is a tentative welding procedure specification that is assumed to be adequate by

the manufacturer but has not been approved.

•Welding Procedure TestInvolves the production and testing of a welded joint in order to prove the feasibility

of a welding procedure.

•Welding Procedure Approval Record (WPAR)A certificate that states all the relevant data / results from a welding procedure test.

•Welding Procedure Specification (WPS)A document that details the variables required to ensure repeatability of a specific

application.

•Welder Approval TestInvolves the production and testing of a welded joint in order to assess the capability

of a welder.

1.3 Welding standards commonly used in the United Kingdom

The Standards listed below are concerned with approval by a testing route:

• BS EN 287-1:2011 - Qualification test of welders - Fusion welding - Steels.

• BS EN ISO 9606 series - Qualification test of welders - Fusion welding.

• BS EN ISO 15614 series - Specification and qualification of welding procedures for

metallic materials - Welding procedure test.

• BS EN 1418:1998 - Welding personnel - Approval testing of welding operators for

fusion welding and resistance weld setters for fully mechanized and automatic

welding of metallic materials.

Other Standards e.g. BS 4872 parts 1 and 2 - Specification for approval testing of welders

when welding procedure approval is not required, remain current.

Page 5: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

5 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

2.0 OBTAINING WELDING CERTIFICATION

There are five key steps to obtaining certification of an approved welding procedure or

an approved welder:

• Preparation of a pWPS or WPS,

• Welding a testpiece,

• Testing,

• Assessment of the results,

• Issue of certification.

Welding and testing will be witnessed by an examining body, normally a third party

inspecting authority, which will then assess the results and issue the certification.

2.1 The first steps

Access to contract documentation to determine what Standards are involved and the

range of approval (material thickness, diameter etc.) is the required first step.

In some EU countries, additional testing requirements are imposed by product Standards

and it is essential that these are also considered at this stage.

It is recommended that SAFed member companies become involved at this stage to provide

advice and guidance based on knowledge of the product and welding Standards involved.

A programme of approvals can then be planned to accord with the contract and provide

maximum coverage for any future contracts. This is an important issue as welding

approvals are valuable documents that can be used on many contracts.

2.2 Essential preparation

It is vital that, prior to the SAFed member company representative (engineer

surveyor) arriving to witness the welding of testpieces, the manufacturer undertakes

adequate preparation.

The minimum requirement is a pWPS detailing the welding parameters necessary for the

welder to weld the testpiece satisfactorily.

Testpieces and consumables should be correctly prepared and stored, and the welder

briefed regarding his role in the approval process e.g. whether it is procedure approval or

welder approval only.

Preferably, some development testing will have been completed to ensure both that the

procedure will be acceptable and/or that the welder has undergone sufficient training.

The better the preparation, the greater the chance that failures, delays and associated

additional costs will be avoided.

Page 6: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

6 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

2.3 Examining bodies

The Examining Body is an organisation appointed to verify compliance with the Standard.

In cases where contracting parties are involved the Examining Body must be acceptable to

those parties.

Acceptability varies between industrial sectors and it is therefore recommended that an

Examining Body which holds national recognition and international notifications

(approvals) and/or affiliations is chosen.

Where authority to issue welding certification is not fully defined by legislation, the major

UK Examining Bodies generally utilise notification under relevant European Union (EU)

Directives as the criteria by which to assess potential Examining Bodies. This approach

provides assurances of the Examining Body's quality system, technical competence in the

relevant technology and adequacy of liability insurance.

SAFed members adopt the above approach to assess the capability of members and other

bodies to issue welding certification.

The United Kingdom Accreditation Service (UKAS) is the sole national accreditation body

recognized by government to assess, against internationally agreed standards.

Organizations that provide welding certification and testing should have this described in

their details of accreditation.

Page 7: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

7 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

3.0 WELDING OF TESTPIECES

3.1 Procedures and parties involved

A SAFed member company selected to conduct welding approvals should be contacted so

that a suitable date and time for welding to proceed can be arranged.

Upon arrival al the site, the engineer surveyor will carry out the following activities:

• Identification of materials against relevant certification,

• Witnessing the set up of the testpiece(s),

• Verification of the welder's identity,

• Marking the testpiece with the relevant identification e.g. Examiner, Welder, pWPS,

• Witnessing the welding of the testpiece,

• Confirming adherence to the Welding Procedure Specification or recording

any differences.

The engineer surveyor may not be present throughout all the welding operation although

for welding procedure testing he is likely to be there.

During the approval lest, the welder will be expected to show adequate practical

experience and knowledge of the welding process, materials and safety requirements for

which approval is being sought.

On completion of welding, the SAFed member company representative will visually

examine the testpiece for compliance with the relevant Standard.

3.2 Job knowledge testing

Testing a welder's job knowledge is optional in BS EN 287, but it may be specifically

required by some European countries.

Job knowledge testing can be performed by SAFed member companies and would be an

additional activity carried out by the engineer surveyor.

Page 8: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

8 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

4.0 TESTING

Following welding and visual examination, tcstpieces will need to undergo non-destructive

and/or destructive testing. Such testing may be undertaken in a SAFed member company

laboratory or by other organisations with suitable facilities and established expertise in

the requirements of welding and product Standards.

If the testing is undertaken by another organisation, the SAFed member company

engineer surveyor would attend the laboratory to witness, as a minimum, the tests that

cannot be verified on examination of testpieces e.g. tensile and impact tests and to assess

other completed tests e.g. radiography, bend and hardness tests.

The SAFed member company engineer surveyor will also assess all the documentation

e.g. material identification, record of welding and test results and take a decision on

compliance with the Standard.

Suitable facilities are provided by laboratories accredited by the United Kingdom

Accreditation Service (UKAS) against the requirement of ISO/IEC 17025:2005 - General

requirements for the competence of testing and calibration laboratories.

Page 9: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

9 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

5.0 CERTIFICATION

5.1 Description of certification

When Certification is issued by the SAFed member company that witnessed the welding

approvals, it will be in a standard formal bearing the SAFed logo and watermark, the

member company's name and a unique identifying number.

The certificates contain translations on the reverse side as an aid to acceptability overseas

and their format has been agreed within CEOC the European Federation.

If manufacturers wish to use their own certificates, such certificates will be endorsed by a

SAFed member company provided they are typed/laser printed, technically and factually

correct and contain all data required by the relevant Standard.

In all cases, certification will only be issued on satisfactory completion of the approval

process and will only be valid when bearing the SAFed member company stamp, signature

and unique identifying number.

5.2 Validity and renewal of certification

Welding Procedures, once approved, remain valid indefinitely and are thus valuable

documents.

For the most common Welder Approval Standard in the United Kingdom, BS EN 287,

the certificate remains valid for two years from the date when all the tests have been

satisfactorily completed, provided it is endorsed by the welding coordinator or the

responsible personnel of the employer at six-monthly intervals.

It is necessary for the welder to have maintained his/her skill and been employed with

reasonable continuity in that class of welding throughout the period of validity to enable

his/her certificate to be endorsed.

If these conditions are not fulfilled the approval lapses automatically.

At the end of the two year period the approval may be renewed (prolongation) by a

SAFed member company after review of the records retained on file with the welder's

approval certificate.

The records of tests must:

• Involve volumetric testing,

• Be traceable to the welder,

• Be representative of the range of approval indicated by the certificate.

If such records arc not available then re-approval will be required. Re-approval at

two-yearly intervals may be found to be more economic than collating and maintaining

records of tests for each welder approval certificate.

Page 10: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

10 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

6.0 SAFed MEMBER COMPANY SERVICES

• SAFed member companies arc major providers of Welding Approvals in the UK.

Considerable experience and expertise is available to make the whole process of

obtaining welding and welder approvals easier for manufacturers.

• SAFed member companies arc able to give expert advice prior to approval on matters

such as:

• Product and Welding Standards,

• Test programmes,

• Development of procedures,

• Advice on training matters.

• This not only ensures technical accuracy but reduces costs and maximises the future

worth of the approvals gained.

• SAFed member companies, via a nation-wide network of engineer surveyors, are able

to deal with all aspects of welding approvals including:

• Witnessing,

• Testing,

• Issue of Certification.

• SAFed member companies have considerable involvement in the drafting and

production of British and European Welding Approval Standards, thus providing the

ability to give advice on known or anticipated future developments.

• SAFed has a technical committee infrastructure that assists uniform application of the

relevant Standards and provides authoritative interpretations of key issues within the

Standards to aid the fabrication industry.

Page 11: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

11 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

APPENDIX I

Welding procedure and welder approval certification

It is essential, for the validity of the certificates, that the details entered areaccurate and complete. (Examples of correctly completed certificates are shown in

the next section).

Welding certificates, correctly completed, potentially span many projects and can

therefore have a long life: they are valuable documents and their accuracy is of the

utmost importance.

Welding Procedure and Welder Approval Certification takes the form of one, or a

combination of, the following:

• El - Welding procedure approval test certificate (optional)This provides formal certification for a welding procedure approval test and a

statement defining the range of approval for essential variables. (See page 12)

• E2 - Details of weld testThis certificate records the actual welding parameters used for the test. It would

always be used in the case of a welding procedure test and possibly for a welder

approval test not carried out to a previously approved procedure. (See page 13)

A continuation sheet E2c is available. (See page 14)

• E3 - Test resultsThis certificate is used to record the results of non-destructive and laboratory tests on

the weld testpiece. It would be used for procedure approval tests without exception,

but for welder approval tests is not normally necessary since test result acceptability is

simply recorded on the Welder Approval Test Certificate (E4). Additional information,

for example photomacrographs or radiographic reports, may need to be appended to

this sheet as applicable. (See page 15)

• E4 - Welder approval test certificateFor most applications this single certificate will include details of the weld test

parameters, the test results and the range of approval. (See page 16)

Certificates E1 - E4 supplied by SAFed have translation details on the reverese for use

if necessary.

Page 12: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

12 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

Page 13: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

13 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

Page 14: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

14 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

Page 15: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

15 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

Page 16: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

16 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

Page 17: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

17 of 18

Welding procedures and welders

Guidelines on approval testing

Edition 2 - November 2012

APPENDIX II

Comparison of numbering systems for welding procedure and welder approval standards

BS EN 287 - Approval testing of welders for fusion welding

Original number Title New number

BS EN 287-1 Steels BS EN ISO 9606-1 *

BS EN 287-2 Aluminium and its alloys BS EN ISO 9606-2

* BS EN 150 9606-1 is not yet a Harmonised European Standard (it is published),therefore, it has not fully replaced BS EN 2871-1: 2011.

BS EN 288 - Specification and approval of welding procedures for metallic materials

Original number Title New number

BS EN 288-1 General rules for fusion welding BS EN ISO 15607

B5 EN 288-3 Welding procedure tests for the BS EN ISO 15614-1

arc welding of steels

BS EN 288-4 Welding procedure tests for BS EN ISO 15614-2

aluminium and its alloys

BS EN 288-8 Approval by a pre-production BS EN ISO 15613

welding test

Page 18: Guidelines on approval testing - SAFed · •Preliminary Welding Procedure Specification (pWPS) This is a tentative welding procedure specification that is assumed to be adequate

Safety Assessment FederationUnit 4, First Floor70 South Lambeth RoadVauxhallLondonSW8 1RL

www.safed.co.uk


Recommended