1
WPS NO. : W GT SM - 1.1 - 002 DATE : NOV. 23, 2011.
REVISION NO. : 0 DATE : NOV. 23, 2011.
SUPPORT PQR NO. : Q GT SM - 1.1 - 002
WELDING PROCESS : GTAW + SMAW TYPE : MANUAL
JOINT DESIGN(QW402)이음 설계 JOINT DETAIL 이음 상태
TYPE OF JOINT GROOVE *** SEE APPLICABLE DRAWING
이음 형태 ROOT FACE ; 2.4±0.8 mm
BACKING ROOT GAP ; MAX. 3.2 mm
백킹 유무
BACKING MAT'L(TYPE)
백킹 재질(형태)
RETAINERS NO V
리테이너 유무
BASE METAL(QW403) 모 재
P NO. 1 Gr NO. 1&2 TO P NO. 1 Gr NO. 1&2 MIN. PREHEAT TEMP
SPEC. TYPE AND GRADE 최저 예열 온도
TO SPEC. TYPE & GRADE MAX. INTERPASS TEMP
사 양 최대 패스간 온도
QUALIFIED THICKNESS RANGE 검정 두께 범위 PREHEAT MAINTENANCE
BASE METAL 5 ~ 25.4 mm 예열 유지
모 재 POST WELD HEAT TREATMENT(QW407) 후열처리
DEPOSIT WELD METAL GT ; 9mm SM ; 16.4 mm
용착 금속 POSTWELD HEAT TREAT. TEMP. NONE
PIPE DIAMETER RANGE ALL 후열처리 온도
관 직경 범위 HOLDING TIME RANGE NONE
MAX. PASS THICK. LIMIT GT ; 3mm, SM ; 5mm 유지 시간
회당 최대 두께 제한 GAS(ES)(QW408) 가 스
FILLER METALS(QW404) 용가재
SHIELDING GAS(ES) GT ; Ar
F NO. A NO. 가스 종류
SFA NO. PERCENT COMPOSITION(MIXTURE) 99.99%
AWS CLASS 혼합가스 조성비율
FLOW RATE
OTHERS 가스 유량
기 타 GAS BACKING NONE
SIZE OF FILLER METAL GT ; ¢2.4 , 3.2 SM ; ¢3.2, 4.0 가스 백킹
용가재 크기 TRAILING GAS NONE
WIRE FLUX CLASS(TYPE) N/A 트레일링 가스
와이어 플럭스 사양(형태) ELECTRCAL CHARACTERISTICS(QW409) 전기 특성
FLUX(FILLER) TRADE NAME N/A
프럭스(필러) 상표명 CURRENT AC OR DC GT ; DC SM ; ACDC
CONSUMABLE INSERT NONE 전 류
소모성 인서트 POLARITY GT ; SP SM ; N/ARP
(NO SUPPLEMENTARY FILLER METALS ARE USED) 극 성
POSITION(QW405) 자 세 TUNGSTEN ELECTRODE TYPE GT ; EWTH-1 OR 2
텅스텐 전극봉 형태
POSITION OF GROOVE TUNGSTEN ELECTRODE SIZE GT ; Φ2.4 , Φ3.2, Φ4
그루우브 자세 텅스텐 전극봉 크기
POSITION OF FILLET MODE OF METAL TRANSFER FOR GMAW
필렛 자세 용융금속 전이 형태 None
PROGRESSION UP DOWN - Pulsing current (GTAW)
진행 방향
양식Q-C0902-1A(0) A4(210x297)mm
NONE
T≤25 mm ; 10 ℃
T>25 mm ; 90 ℃
200 ℃
PREHEAT(QW406) 예 열
- APPLICABLE CODE : ASME SEC.I
PAGE : 1 OF 2
W GT SM - 1.1 - 002WELDING PROCEDURE SPECIFICATION용 접 작 업 표 준 (WPS)
1
NOTE 1
YES - NO V
GT ; ER70S-6 SM ; E7016
GT ; 5.18 SM ; 5.1
YES -
WELD METAL & BASE METAL
GT ; 6 SM ; 4
NOTE 1
GTAW (solid wire)
ALL
ALL
V
GT ; 8~14 L/min
APPLICABLE CODE : ASME SEC. Ⅸ
Victaulic L.L.C
2
WELDING TECHINIQUE(QW410) 용접 기법 METHOD OF BACK GOUGING
가우징 방법 None
STRINGER OR WEAVE BEAD BOTH SINGLE OR MULTIPLE PASS(PER SIDE)
비드 형태 단층 혹은 다층 MULTIPLE
ORIFICE OR GAS CUP SIZE GT ; 3/8"~5/8" OSCILLATION
가스컵 크기 진 동 None (GT) , N/A (SM)
INITIAL OR INTERPASS CLEANING GRINDING SINGLE OR MULTIPLE ELECTRODE
초층/층간 청결 방법 OR BRUSHING 단극 혹은 다극 SINGLE
CONTACT TUBE TO WORK DIST. N/A PEENING
접촉관과 용접물간 거리 피이닝 NONE
NOTE 1
AWS NO.
GTAW SMAW
TO
*** SPECIAL NOTE 특기사항
1. ANY P-NO.1 OR EQUIVALENT MATERIAL IN QW-422 OF ASME SECTION IX.
2. MAX WEAVE PASS SHALL NOT EXCEED 2 TIMES OF THE ELECTODE CORE DIA.
양식Q-C0902-1B(0) A4(210x297)mm
PAGE : 2 OF 2
REMARKS
10~20 10~20
22~30 15~20
VOLTS TRAVEL
OTHERRANGE
S.H. KIM
REVIEWED BY
A516-60
A106
A53 GR B
A105
J. H. LEE K. W. LEE
REVIEWED BY
A516-60
A106
ER70S-6 E7016
PREPARAED BY APPROVED BY
BASE METAL
80~140
CLASS
1 st
12~18SMAW ¢3.2
LAYER NO. PROCESS
10~15
(mm)
DIA.
110~160
W GT SM - 1.1 - 002WELDING PROCEDURE SPECIFICATION
CLASS
용 접 작 업 표 준 (WPS)
DCRP
(A)
AMP RANGE
GTAW
¢3.2
CURRENT
TYPE POLAR
TABLE 1
DCSP
120~200REST SMAW TABLE 1 ¢4.0 DCRP
A53 GR B
A105
TABLE 1
TABLE 12 nd
3 rd
GTAW
¢2.4
SPEED
(V) (cm/min)
20~25100~180
6~18
A234 WPB
Victaulic L.L.C
A234 WPB
DCSP
3
2
1
4
3
PQR NO. : Q GT SM - 1.1 - 002 DATE : NOV. 23, 2011.
WPS NO. : W GT SM - 1.1 - 002
WELDING PROCESS : GTAW + SMAW TYPE : MANUAL
JOINT DESIGN USED
BASE METAL(QW403) 모 재 PERHEAT(QW406) 예 열
SPEC. TYPE AND GRADE A106 GR B/A53 GR B PREHEAT TEMP. 20 ℃
INTERPASS TEMP. 200 ℃
TO SPEC. TYPE & GRADE A106 GR B/ A53 GR B OTHER N/A
P NO. 1 Gr NO. 1 TO P NO. 1 Gr NO. 1 POST WELD HEAT TREATMENT(QW407) 후열처리
BASE METAL 12.7 mm TEMPRATURE None
HOLDING TIME None
PIPE DIAMETER 8" SCH80 OTHER None
DEPOSIT WELD METAL TH'K GT ; 4.5 mmSM ; 8.2 mm GAS(ES)(QW408) 가 스
FILLER METALS(QW404) 용가재 TYPE OF GAS(ES) GT ; Ar
PERCENT COMPOSITION(MIXTURE) 99.99%
WELD METAL ANALYSIS A NO. GT ; 1 SM ; 1 FLOW RATE GT ; 8~14 L/min
SIZE OF ELETRODE GT ; ¢2.4, 3.2 SM ; ¢3.2, 4.0 ELECTRCAL CHARACTERISTICS(QW409) 전기 특성
FILLER METAL F NO. GT ; 6(SOLID) SM ; 4 CURRENT AC OR DC GT ; DC SM ; ACDC
POLARITY GT ; SP SM ; N/ARP
SFA SPECIFICATION GT ; 5.18 SM ; 5.1 TUNGSTEN ELECTRODE TYPE GT ; EWTH-2
TUNGSTEN ELECTRODE SIZE GT ; ¢2.4
AWS CLASSIFICATION GT ; ER70S-6 SM ; E7016
TECHNIQUE(QW410) 용접 기법
FLUX TRADE NAME N/A
(FILLER) STRINGER OR WEAVE BEAD BOTH
POSITION(QW405) 자 세 OSCILLATION None (GTAW)
POSITION OF GROOVE 6G SINGLE OR MULTIPLE PASS(PER SIDE)
MULTIPLE
POSITION OF FILLET -
SINGLE OR MULTIPLE ELECTRODE SINGLE
WELD PROGRESSION UPHILL
OTHER N/A
OTHER NONE
양식Q-C0902-2A(0) A4(210x297)mm
PAGE : 1 OF 2
Q GT SM - 1.1 - 002
9.5
E7016 ¢4.0 160
13 11.17
INPUT
(KJ/Cm)
10.6713
18.3 13.6426
110 22E7016 ¢3.2
12
ER70S-6 ¢3.2 130
7.3 11.84
HEAT
Victaulic L.L.C
REST SMAW
2 GTAW
3 SMAW
(A) (V)
¢2.4 120
ELECTRODE SIZE
AMPS
ER70S-6
(Cm/min)
1 GTAW
SPEEDBEAD NO. PROCESS
VOLT TRAVEL
RANGE RANGE
PROCEDURE QUALIFICATION RECORD용접 절차 인증기록서 (PQR)
APPLICABLE CODE : ASME SEC. Ⅸ
2
1
2
43
4
TENSILE TEST (QW150) : Tested(TAS-039453)
GUIDED BEND TEST (QW160) : Tested(TAS-39453)
TOUGHNESS TEST (QW170) : Tested(TAS-39453)
1 2 3
FILLET WELD TEST (QW180) : N/A
RESULT-SATISFACTORY : YES NO PENETRATION INTO PARENT METAL : YES NO
TYPE AND CHARACTER OF FAILURE MACRO-RESULTS
Speicmen No WELD METAL
OTHER TEST :
RADIOGRAPHIC TEST Refer To Attacment ( RT Report No. : ITEC-SC-RT-1111-001 )
DEPOSIT ANALYSIS
MACRO TEST Refer To Attacment ( TAS-39453 : Photo )
MICRO TEST Refer To Attacment ( TAS-39453 : Photo )
OTHER
WELDER'S NAME : STAMP NO. : SC-W-06
TEST CONDUCTED BY : J. S. MOON TEST REPORT NO. : TAS-39453
WE CERTIFY THAT THE STATEMENTS IN THIS RECORD ARE CORRECT AND THAT THE TEST WELDS WERE
PREPARAED, WELDED, AND TESTED IN ACCORDANCE WITH THE REQUIREMENTS OF ASME SECTION IX.
양식Q-C0902-2B(0) A4(210x297)mm
NO3
NO1
NO2
163
389 390
HAZ
178
176
181 194
BASE METAL
161
164
REMARK
193
197
10 * 10 * 55
REMARKS
10 * 10 * 55
Q GT SM - 1.1 - 002
386 369
STRESS(N/mm²) AND LOCATION
471 Ductile, Base Metal
IMPACT VALUE (J)
477 Ductile, Base Metal
ULTIMATE UNIT TYPE OF FAILURE
PROCEDURE QUALIFICATION RECORD용접 절차 인증기록서 (PQR)
REVIEWED BY
- 29
TYPE (℃)
- 29
V
V 40 36
HARDNESS TEST (HV): TEST LOAD: 10kgf / Tested(TAS-339453)
J. H. LEE K. W. LEE
V - 29HAZ
BASE METAL
PREPARAED BY REVIEWED BY CERTIFIED BY
S.H. KIM
TYPE AND FIGURE NO.
FACE BEND(QW-462.3(a)) F1
RESULT
ACCEPTED (PASS)
FACE BEND(QW-462.3(a)) F2
ROOT BEND(QW-462.3(a)) R1
ACCEPTED (PASS)
ACCEPTED (PASS)
112.369NO. 2 19.06 12.35 235.39
TOTAL LOAD(kN)
NO. 1 19.11 11.50 219.76 103.436
NO. (MM) (MM) (mm²)
PAGE : 2 OF 2
SPECIMEN WIDTH THICK'S AREA ULTIMATE
No.3
SPECIMEN
NO.
No.1
TEST TEMP.NOTCH
38
10 * 10 * 55383
Victaulic L.L.C
Seong-Gi, Hong
No.2
WELD
ROOT BEND(QW-462.3(a)) R2
NOTCH
LOCATION
ACCEPTED (PASS)
392