1
Materials for sintered oil-retaining bearings DIN 30910-3:2004-11 Material Abbrevi- ation Permissible ranges Representive examples Density a Porosity Chemical composition (mass share) Radial breaking strength Hard- ness Density a Porosity Chemical composition (mass share) Radial breaking strength Upsetting boundary Hard- ness Heat con- ductivity Sint- ρ x 100 C Cu Sn Fe others K C HB ρ x 100 b C Cu Sn Fe others K C ς d 0,2 HB C גg/cm 3 % % % % % % N/mm 2 g/cm 3 % % % % % N/mm 2 N/mm 2 W/mK Sintered iron A 00 B 00 C 00 5,6 – 6,0 6,0 – 6,4 6,4 – 6,8 25 ± 2,5 20 ± 2,5 15 ± 2,5 <0,3 < 1,0 Re- mai- ning < 2 > 150 > 180 > 220 > 25 > 30 > 40 5,9 6,3 6,7 25 20 15 Re- mai- ning < 0,2 160 190 230 130 160 180 30 40 50 37 43 48 Sintered steel cupriferous A 10 B 10 C 10 5,6 – 6,0 6,0 – 6,4 6,4 – 6,8 25 ± 2,5 20 ± 2,5 15 ± 2,5 <0,3 1 5 Re- mai- ning < 2 > 160 > 190 > 230 > 35 > 40 > 55 5,9 6,3 6,7 25 20 15 2,0 Re- mai- ning < 0,2 170 200 240 150 170 200 40 50 65 36 37 42 cupriferous and carbo- niferous B 11 6,0 – 6,4 20 ± 2,5 0,4 1,5 1 5 Re- mai- ning < 2 > 270 > 70 6,3 20 0,6 2,0 Re- mai- ning < 0,2 280 160 80 28 higher cup- riferous A 20 B 20 5,8 – 6,2 6,2 – 6,6 25 ± 2,5 20 ± 2,5 <0,3 15 25 Re- mai- ning < 2 > 180 > 200 > 30 > 45 6,6 6,4 25 20 20,0 Re- mai- ning < 0,2 200 220 140 160 40 50 41 47 higher cupr- and carboni- ferous A 22 B 22 5,5 – 6,0 6,0 – 6,54 25 ± 2,5 20 ± 2,5 0,5 3,0 15 25 Re- mai- ning < 2 > 120 > 140 > 20 > 25 5,7 6,1 25 20 2,0 d 20,0 Re- mai- ning < 0,2 125 145 100 120 25 30 30 37 Sintered bronze A 50 B 50 C 50 6,4 – 6,8 6,8 – 7,2 7,2 – 7,7 25 ± 2,5 20 ± 2,5 15 ± 2,5 < 0,2 Re- mai- ning 9 11 < 2 > 120 > 170 > 200 > 25 > 30 > 35 6,6 7,0 7,4 25 20 15 Re- mai- ning 10,0 < 0,2 140 180 210 100 130 160 30 35 45 27 32 37 graphit- iferous e A 51 B 51 C 51 6,0 – 6,5 6,5 – 7,0 7,0 – 7,5 25 ± 2,5 20 ± 2,5 15 ± 2,5 0,5 3,0 Re- mai- ning 9 11 < 2 > 100 > 150 > 170 > 20 > 25 > 30 6,3 6,7 7,1 25 20 15 1,5 e Re- mai- ning 10,0 < 0,25 120 155 175 80 100 120 20 30 35 20 26 32 a Non-impregnated Coefcient of thermal expansion a (independent of density) b The Oil content amounts to no less than 90 % of the open porosity Sintered iron and steel: a ~ 12 x 10 -6 /K c Measured on the calibrated bearings Ø 10/16 x 10 Sintered bronze: a ~ 18 x 10 -6 /K d C occurs primarily as free graphite e C occurs as free graphite Δ V V Δ V V

Materials DIN Sim Sinterformteile Tabelle e2

Embed Size (px)

DESCRIPTION

Materials DIN Sim Sinterformteile Tabelle e2

Citation preview

  • Materials for sintered oil-retaining bearings DIN 30910-3:2004-11

    Material

    Abbrevi-ation

    Permissible ranges Representive examples

    Densitya Porosity Chemical composition(mass share)Radial

    breaking strength

    Hard-ness Density

    a Porosity Chemical composition(mass share)Radial

    breaking strength

    Upsetting boundary

    Hard-ness

    Heat con-ductivity

    Sint- x 100 C Cu Sn Fe others KC HB x 100b C Cu Sn Fe others KC d 0,2 HB

    C

    g/cm3 % % % % % % N/mm2 g/cm3 % % % % % N/mm2 N/mm2 W/mK

    Sintered ironA 00B 00C 00

    5,6 6,06,0 6,46,4 6,8

    25 2,520 2,515 2,5

    < 0,3 < 1,0Re-mai-ning

    < 2> 150> 180> 220

    > 25> 30> 40

    5,96,36,7

    252015

    Re-mai-ning

    < 0,2160190230

    130160180

    304050

    374348

    Sintered steel

    cupriferousA 10B 10C 10

    5,6 6,06,0 6,46,4 6,8

    25 2,520 2,515 2,5

    < 0,31 5

    Re-mai-ning

    < 2> 160> 190> 230

    > 35> 40> 55

    5,96,36,7

    252015

    2,0Re-mai-ning

    < 0,2170200240

    150170200

    405065

    363742

    cupriferous and carbo-

    niferousB 11 6,0 6,4 20 2,5

    0,4

    1,5

    1 5

    Re-mai-ning

    < 2 > 270 > 70 6,3 20 0,6 2,0Re-mai-ning

    < 0,2 280 160 80 28

    higher cup-riferous

    A 20B 20

    5,8 6,26,2 6,6

    25 2,520 2,5 < 0,3

    15 25

    Re-mai-ning

    < 2 > 180> 200> 30> 45

    6,66,4

    2520 20,0

    Re-mai-ning

    < 0,2 200220140160

    4050

    4147

    higher cupr- and carboni-

    ferous

    A 22B 22

    5,5 6,06,0 6,54

    25 2,520 2,5

    0,5

    3,0

    15 25

    Re-mai-ning

    < 2 > 120> 140> 20> 25

    5,76,1

    2520 2,0

    d 20,0Re-mai-ning

    < 0,2 125145100120

    2530

    3037

    Sintered bronze

    A 50B 50C 50

    6,4 6,86,8 7,27,2 7,7

    25 2,520 2,515 2,5

    < 0,2Re-mai-ning

    9 11

    < 2> 120> 170> 200

    > 25> 30> 35

    6,67,07,4

    252015

    Re-mai-ning

    10,0 < 0,2140180210

    100130160

    303545

    273237

    graphit-iferous e

    A 51B 51C 51

    6,0 6,56,5 7,07,0 7,5

    25 2,520 2,515 2,5

    0,5

    3,0

    Re-mai-ning

    9 11

    < 2> 100> 150> 170

    > 20> 25> 30

    6,36,77,1

    252015

    1,5eRe-mai-ning

    10,0 < 0,25120155175

    80100120

    203035

    202632

    a Non-impregnated Coeffi cient of thermal expansion a (independent of density)b The Oil content amounts to no less than 90 % of the open porosity Sintered iron and steel: a ~ 12 x 10 -6/Kc Measured on the calibrated bearings 10/16 x 10 Sintered bronze: a ~ 18 x 10 -6/Kd C occurs primarily as free graphitee C occurs as free graphite

    VV

    VV