ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking P. Scott FRAME TOME, Tour Fiat Cedex 16, 92084 Paris la De-fense, France Received 21 December 1993; accepted 26 April 1994 Abstract The aim of this review is to assess from the available data whether irradiation in PWR primary water can adversely affect the properties of stainiess steels due to irradiation assisted stress corrosion cracking (IASCC). The following aspects are examined: (i) Irradiation damage of the material. (ii) The influence of water radiolysis. Since the irradiation damage processes are similar for both PWR and BWR systems, differences observed in the intergranular cracking properties of core components of both systems must be attributable to differences in the synergistic interactions with the coolant chemistry. These aspects are analysed in detail to determine to what extent BWR experience can be used to predict IASCC in PWR core components. Several related potential failure mechanisms are also reviewed such as radiation hardening, radiation creep and helium or hydrogen embrittlement. The probable role of some or all of these failure mechanisms in core component failures observed to date, and in experiments ostensibly designed to observe IASCC, is critically examined. 1. Introduction Irradiation assisted stress corrosion cracking (IASCC) is a term which has been used in recent years to describe intergranular cracking showing little or no ductility which can occur in heavily irradiated struc- tural components of nuclear reactor cores. Since irradi- ation by high energy neutrons can affect both the material properties and the environmental chemistry and y rays can also influence the latter, IASCC is a complex problem which is neither easy to investigate practically nor simple to understand mechanistically. Indeed in some cases, as we shall see, both in compo- nent failures and experimental investigations, it is not always certain that corrosion played a significant role while in others irradiation may only be of secondary importance in providing localized superheat to concen- trate dissolved salts. A major review of the present state of knowledge of IASCC has recently been published [I] and subse- quently updated [2]. Like much of the literature cited therein, including published incidents of cracking of stainless steel core components, the review is written largely from the perspective of designers and operators of boiling water reactors (BWRS). No attempt has yet been made, so far as is known, to review the topic with a pressurized water reactor (PWR) perspective which is the objective of this paper. Iiistorically, since the advent of nuclear power reac- tors, there have been sporadic reports of intergranular fractures in highly irradiated stainless steels (and nickel base alloys). A summary is given in Table 1 with appropriate references [l-9]. The first incidents were in early examples of stainless steel fuel cladding both for PWRs and BWRs although much less severe in the former case [3,4]. This problem was apparently im- proved significantly by reducing the silicon and phos- phorus contents below 0.1 and 0.01% respectively and then avoided altogether by the almost universal adop- tion of zircaloy fuel cladding. Nevertheless, even today, irradiated stainless steel fuel cladding of advanced gas cooled reactors (AGRs) has suffered from IASCC fail- ures following discharge to the fuel cooling ponds [l]. Potential problems with IASCC of stainless steel water Eisevier Science B.V. .sSL)I 0022-3115(94)00301-4

A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

  • Upload
    others

  • View
    5

  • Download
    0

Embed Size (px)

Citation preview

Page 1: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

ELSEVIER Journal of Nuclear Materials 211(1994) 101-122

Review article

A review of irradiation assisted stress corrosion cracking

P. Scott

FRAME TOME, Tour Fiat Cedex 16, 92084 Paris la De-fense, France

Received 21 December 1993; accepted 26 April 1994

Abstract

The aim of this review is to assess from the available data whether irradiation in PWR primary water can adversely affect the properties of stainiess steels due to irradiation assisted stress corrosion cracking (IASCC). The following aspects are examined: (i) Irradiation damage of the material. (ii) The influence of water radiolysis. Since the irradiation damage processes are similar for both PWR and BWR systems, differences observed in the intergranular cracking properties of core components of both systems must be attributable to differences in the synergistic interactions with the coolant chemistry. These aspects are analysed in detail to determine to what extent BWR experience can be used to predict IASCC in PWR core components. Several related potential failure mechanisms are also reviewed such as radiation hardening, radiation creep and helium or hydrogen embrittlement. The probable role of some or all of these failure mechanisms in core component failures observed to date, and in experiments ostensibly designed to observe IASCC, is critically examined.

1. Introduction

Irradiation assisted stress corrosion cracking (IASCC) is a term which has been used in recent years to describe intergranular cracking showing little or no ductility which can occur in heavily irradiated struc- tural components of nuclear reactor cores. Since irradi- ation by high energy neutrons can affect both the material properties and the environmental chemistry and y rays can also influence the latter, IASCC is a complex problem which is neither easy to investigate practically nor simple to understand mechanistically. Indeed in some cases, as we shall see, both in compo- nent failures and experimental investigations, it is not always certain that corrosion played a significant role while in others irradiation may only be of secondary importance in providing localized superheat to concen- trate dissolved salts.

A major review of the present state of knowledge of IASCC has recently been published [I] and subse- quently updated [2]. Like much of the literature cited therein, including published incidents of cracking of

stainless steel core components, the review is written largely from the perspective of designers and operators of boiling water reactors (BWRS). No attempt has yet been made, so far as is known, to review the topic with a pressurized water reactor (PWR) perspective which is the objective of this paper.

Iiistorically, since the advent of nuclear power reac- tors, there have been sporadic reports of intergranular fractures in highly irradiated stainless steels (and nickel base alloys). A summary is given in Table 1 with appropriate references [l-9]. The first incidents were in early examples of stainless steel fuel cladding both for PWRs and BWRs although much less severe in the former case [3,4]. This problem was apparently im- proved significantly by reducing the silicon and phos- phorus contents below 0.1 and 0.01% respectively and then avoided altogether by the almost universal adop- tion of zircaloy fuel cladding. Nevertheless, even today, irradiated stainless steel fuel cladding of advanced gas cooled reactors (AGRs) has suffered from IASCC fail- ures following discharge to the fuel cooling ponds [l]. Potential problems with IASCC of stainless steel water

Eisevier Science B.V. .sSL)I 0022-3115(94)00301-4

Page 2: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

102 P. Scott /Journal of Nuclear Materials 211 (1994) 101-122

Table 1 Intergranular cracking in core components

Core component Material

Fuel cladding T 304 Fuel cladding 20% Cr/25% Ni/Nb

Fuel element component 20% Cr/25% Ni/Nb

Neutron source tubes T 304 Control rod blades, T 304

handles + sheaths

Control rod cladding T 304

Instrument dry tubes T 304

Core spray line and T 304

sparger

Core baffle bolts T 316

Absorber pins I 600

Bolts A 286 thermal shield

fuel assembly

core baffle

Bolts I 600

shroud head I 600

fuel assembly

Bolts and springs IX 750

core baffle

fuel assembly

control rod drive seal

fuel assembly finger

jet pump beams

Control rod guide tube IX 750

support pins

Reactor

BWR and PWR h

AGR a

SGHWR (BWR)

BWR

BWR

PWR

BWR

BWR

PWR

PWR

BWR and PWR

BWR

PWR

BWR and PWR

PWR

Reference

[1,3,41

[II

[II

[II

[I,41

II,6-81

[ll

[71

[7,91

[41

[I,51

[II

[71

[1,4,5,71

[I,4,5,71

a Cracking occurred in the fuel cooling pond.

h Attributed originally to poor water chemistry.

cooled, first wall components of nuclear fusion reactors are also now being actively investigated [lo].

Examination of these cracking incidents in fuel cladding and more recently PWR control rod cladding has given rise to the proposition of a threshold fast neutron dose for the occurrence of IASCC; - 5 X 102’ n/cm2 (E > 1 MeV) or - 1.0 displacement per atom (dpa) for BWRs and a larger dose - 1 to 2 X 102’ n/cm2 (E > 1 MeV) for PWRs.

Consequently, it is necessary to examine the possi- ble degradation of resistance to intergranular stress corrosion in other highly irradiated stainless steel (or nickel base alloy) core components. These may reach such dose thresholds quoted above much later than fuel or control rod cladding but nevertheless within the design life of the plant. One aim of this review is to examine the validity of these proposed neutron dose thresholds with particular emphasis on PWR compo- nents.

Two features of IASCC which set is apart from other stress corrosion cracking phenomena are the evolution of microstructure with time caused by fast

neutrons and the influence of ionising radiations on the environmental chemistry. Atom displacements from their normal lattice positions in metallic materials not only give rise to progressive hardening and loss of ductility, they also lead to changes in grain boundary composition if the temperature is high enough for diffusion of point defects to take place to natural sinks such as grain boundaries. In addition neutron capture reactions yielding hydrogen and helium may contribute to embrittlement of the material, while dimensional changes due to irradiation induced creep or swelling may significantly change the applied stress. These pro- cesses are likely to be quite similar from one thermal reactor type to another and their consequences for stress corrosion susceptibility, insofar as they are known, are reviewed. The effect of radiation on envi- ronmental chemistry is also reviewed in detail and the fundamental differences between BWR and PWR coolants highlighted with particular reference to their impact on the altered microstructures of irradiated stainless steels (and nickel base alloys).

We start with a review of the environmental chem-

Page 3: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

P. Scott/Journal of Nuclear Materials 211 (1994) 101-122 103

Table 2 Linear energy transfer and yields for reactor irradiations (12)

Radiation type Mean LET (eV/nm)

PT Y 0.1 Fast neutrons 40

G values; yield/100 eV

e-=4 H+ HA OH HO, H H2

2.70 2.70 0.61 2.86 0.03 0.61 0.43 0.93 0.93 0.99 1.09 0.04 0.50 0.88

istry as a necessary background to interpreting the radical reaction products described by the following

observed differences between PWRs and other types of equation.

thermal reactor. H,O + H,, H,O,, e,, H, OH, H+, HO,.

2. Radiolysis effects

2.1. Radiolysis of water

The absorption of ionising radiations by water leads to its dissociation into several molecular, ionic and

These interact in a series of known reactions, most with rather low activation energies of = 3 kcal/mol, forming H,, 0, and H,O, [11,12]. However, the over- all stability of water increases with increasing tempera- ture and yields of molecular decomposition products (H,, 0, and H,O,) are correspondingly reduced.

The concentrations of the primary products of radi-

10-S 2 4 6 810’ 2 4 6810-3 2 4 6 810-Z

lNlT!AL HYDROGEN IN MOLES/KG

Fig. 1. Steady state concentrations of several radiolysis products in PWRs versus the initial hydrogen concentration [13].

Page 4: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

104 P. Scott/Journal of Nuclear Materials 211 (1994) 101-122

olysis are controlled by the linear energy transfer rate (LET) for each radiation type and the reaction yield given by the G values; i.e. the number of molecules, ions or radicals formed for each 100 eV absorbed. G values can vary sharply with the LET so that radiation quality has a significant impact on the primary reaction product concentrations [11,12]. Typical LET and G values for y rays and neutrons are shown in Table 2.

It can be deduced, therefore, that laboratory experi- ments with y rays alone, however powerful, will not reproduce the concentrations, or perhaps more impor- tantly, the correct ratios of primary radiolytic products occurring in power reactors where the majority of the energy absorbed by the water coolant/moderator is due to neutrons.

wherever possible, or at least understand the processes controlling it. Measurement of electrochemical poten- tials is fairly difficult in high temperature water and fraught with problems in nuclear plant, especially in the core. Nevertheless such measurements have been attempted in BWRs and with some success [15-171. Their main objective is to establish a method of relat- ing corrosion potential under irradiation in BWR cores to the results of calculations of water radiolysis so that corrosion potentials around the BWR water circuit may in future be calculated [17].

The influence of solutes on the yields of molecular products also varies strongly between y and neutron radiation [ll]. Solutes reacting readily with eLQ or H, reduce the yield of hydrogen whereas those reacting with OH, reduce the yield of hydrogen peroxide. This effect is observed only weakly under y irradiation but strongly under neutron irradiation. By adding a few ml/kg of hydrogen, as in PWRs, radiolytic dissociation of water is strongly suppressed, Fig. 1 [13], whereas in BWRs without added hydrogen, a concentration of

oxygen of - 200 ppm is observed, the precise value depending on plant design [14]. Hydrogen peroxide is only observed in BWRs if special precautions are taken before analysis to minimize its thermal decomposition as the water exits the core.

Compared to typical corrosion potentials on stain- less steel and nickel alloy components out of core of - - 100 to + 100 mV (SHE), an elevation of potential by as much as 250 mV is observed in BWR cores. Similar measurements have not been attempted in PWR cores.

A key question is then: what are the reasons for the elevation of the electrochemical corrosion potential in BWRs and is a simiiar process possible in PWRs?

Radiation electrochemistry (usually involving only y radiation) has been studied extensively at relatively low temperatures normally accessible in the laboratory [18]. The effects of radiation may be classified according to the location where the radiation is absorbed:

(i) in the bulk solution, (ii) in the interfacial region between solution and

electrode, and (iii) in the electrode itself.

Detailed analysis of the chemical reactions of water undergoing ionising radiations in power reactors has relied mainly on complex computer based calculations using the best available data on known elemental reac- tions. The main check of their efficacy is comparison between predicted and measured yields of molecular decomposition products, O,, H, and H,Oz. The pres- ence of traces of some transition metal ion impurities such as Cuzi and the recently confirmed greater stabil- ity than was previously thought of H,O, at high tem- peratures have not so far been shown to have strong effects. Despite detailed arguments concerning precise quantitative data for individual ion-molecule or radi- cal-molecule reactions, computer codes predicting wa- ter radiolysis effects appear to do quite an effective job. This is particularly so in the context of the com- plexities of two phase flow in BWRs [14]. The PWR primary water situation is much simpler because boil- ing is prevented and water decomposition is effectively suppressed by a hydrogen overpressure [13].

In initially deaerated acidic solutions, the potentials of platinum, stainless steel and nickel behave quite similarly provided there is no significant corrosion and, with the exception of platinum, are controlled com- pletely by diffusion of electrochemically active species from the bulk solution to the electrode surface. (In the case of platinum, absorption of energy by the electrode surface itself also plays a part.) It is observed that potentials fall initially to the reversible hydrogen value despite the simultaneous radiolytic production of hy- drogen peroxide. With increasing dose, potentials are observed to rise to values controlled mainly by hydro- gen peroxide redox reactions because the yield (G value) of peroxide is greater than that of hydrogen.

2.2. Electrochemistry

By contrast, if a hydrogen purge is present in similar low temperature y radiolysis experiments, an efficient radical chain decomposition of peroxide and hydroxide radicals prevents any net change in solution composi- tion and, consequently, any significant change in corro- sion or redox potentials. On platinum, however, the exchange current density for the hydrogen ion reduc- tion reaction is increased by energy absorption by the electrode surface and the potential shifts slightly in the negative direction.

In virtually all aqueous stress corrosion phenomena, Recent experiments to measure the effect of high

the electrochemical corrosion potential is a key con- intensity y radiation on the potentials of platinum and

trolling parameter and it is important to measure it stainless steel in 288°C water have shown the same

Page 5: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

P. Scott /Journal of Nuclear Materials 21 I (1994) 101-122 105

- 0.6

Effect of Radiation on Corrosion Potential of 304 St. Steel & Pt in 288°C Water

A BWR TopCore n +y

V Proton Rad. = BWR Peak

+ 30 - 200 MRad/h y

0 0.3 - 2 MRad/h y

n Pt, various Rad levels

Open symbols = no radiation

Lines indicate paired data (eg. yonloff) Band of data for unirradiated conditions

(a) -

IO' 102 103 104

Dissolved Oxygen, ppb

Shift in Corrosion Potential from irradiation 304 St. Steel & Pt in 288°C Water

L”““’ v’, ’ ’ “““’ ’ “““” ’ ’ “““’ ’ ’ “““’ ’ I’-

\ 200 ppb Hz

2 points BWR Top Core n + y

Proton Rad. q BWR Peak

30 - 200 MRad/h y

0.3 - 2 MRad/h y

Pt, various Rad levels v Proton, ECP in Crevice n

<IO0 10’ 102 103 104

Dissolved Oxygen, ppb

Fig. 2. Effect of radiation on (a) the corrosion potential of type 304 stainless steel in 288°C water (b) the shift in corrosion potential

relative to unirradiated conditions [2].

Page 6: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

106 P. Scott/Journal of Nuclear Material 211 (1994) 101-122

general trends described above for lower temperatures [1,2], Fig. 2. However, only 150 ppb of dissolved hydro- gen was sufficient to suppress any increase in poten- tials during y irradiation.

Immediate extrapolation of trends observed with y irradiation to the much higher power densities and LETS associated with in-core neutron and y irradiation must be treated cautiously. Indeed, there is evidence in pure water and o~genated water that proton irradia- tion which closely simulates the energy deposition and primary radiolytic reaction yields of BWR cores does give rise to greater positive potential shifts on stainless steel and platinum than y irradiation alone {2]. This is corroborated by the measurements of BWR in-core potentials mentioned earlier [1.5-l’?]. Recent theoreti- cal calculations based on a mixed potential model for electrochemical corrosion and redox potentials have reproduced these observations extremely well, Fig. 3

h91. An underlying assumption is that the electrochemi-

cal potential is controlled by diffusion to metal surfaces of the molecular products of radiolysis, H,, 0, and H,O,. This is readily understood from an examination of the relative orders of magnitude of the rate con- stants of elementary ion-molecule reactions and of

typical electrochemical reactions, and also the exceed- ingly low steady state concentrations of ions and radi- cals 112,141. These calculations also demonstrate the importance of fluid dynamics in controlling diffusion rates of electrochemically active species across the boundary layer to the metal surface.

In the presence of excess hydrogen as in PWR primary circuits, as has already been noted, the forma- tion of oxidising species is effectively suppressed [l&13], Fig. 1. Indeed, early experiments in a power PWR into which oxygen was deliberately injected showed that the half-life of oxygen was only 12 min at a power density of 2.5 W/g [ll]. It was further found that the hydrogen concentration had to be reduced well below the speci- fied minimum (25 ml/kg) before oxygen could be de- tected. Therefore, there is no reason to suppose that corrosion potentials in a PWR core would be signifi- cantly different to those out-of-core and must be deter- mined everywhere by the hydrogen ion reduction reac- tion, i.e. -600 to -800 mV (SHE).

Another important question concerning the effects of irradiation on electrochemical potentials is whether any unusual effects could occur in cracks or crevices.

Normally, in the absence of irradiation, the poten- tial of stainless steels or nickel base alloys in a crevice

Lab + in _ plant data type 304 f 316 SS. 266” C

” Calculated using mixed potential model

Re -

GE In-plant (mrc) measurements (Duane Arnold)

I .I//#

0.01 ppm 0.1 Ppm lpPm log. [02] I ppm

( ! I 8

I I I I --- -3 -2 -7 0 +l

Fig. 3. Electrochemical corrosion potential versus oxygen and hydrogen peroxide concentration at 288°C [19].

Page 7: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

P. Scott /Journal of Nuclear Materials 211 (1994) 101-l 22 107

is always low and close to the hydrogen redox value. If oxygenated water and a suitable anion are present at the mouth of the crevice, the crevice pH can shift strongly in the acid direction whereas in the absence of oxygen virtually no change in crevice solution chemistry occurs since there is no driving force, i.e. no potential difference between the crevice mouth and tip.

The available evidence from recent experiments us- ing proton irradiation of a carefully selected energy from a cyclotron to simulate the LETS and G values of neutrons and y rays in a BWR shows that the crevice or crack chemistry is not significantly changed by radi- olysis; i.e. crevice potentials remain near hydrogen redox values independent of the potential outside the crevice [2]. Therefore, there appears to be little risk of any unusual crevice chemistry directly attributable to irradiation in hydrogenated PWR primary water chem- istry.

It is conceivable, however, that the condition above may not be satisfied in closed crevices where local boiling might occur due to y heating and restricted water circulation. Crevices, even closed ones, without boiling are not considered a problem, particularly where there is an initial excess of hydrogen, since there would be no net change in overall composition of the crevice solution on radiolysis. However, the chemical compounds lithium hydroxide and boric acid normally added to PWR primary water could be concentrated significantly by local boiling and lead both to a threat of crevice corrosion as well as stress corrosion cracking (e.g. caustic cracking).

2.3. Stress corrosion cracking

Experimental studies of the influence of irradiation on aqueous environmental effects on stress corrosion cracking of stainless steels (or nickel base alloys) have mainly been designed to investigate BWR conditions. However, some data have been obtained with low oxygen and/or added hydrogen which allow some judgements to be made concerning trends in PWR systems. (Stress corrosion tests on preirradiated mate- rials and in-reactor experiments which simulate both the radiation damage to the material as well as the radiation chemistry of the environment are discussed in later sections.)

The simplest types of experiment on radiation chemistry effects have utilized relatively powerful Co6’ y sources [1,2,20,21], albeit at least three orders of magnitude less intense than in the core of a nuclear reactor. Slow strain rate tests have been carried out on type 304 stainless steel with prior thermal sensitization of the grain boundaries (to produce grain boundaries with chromium depletion). As deduced in the preced- ing sections, the electrochemical potential of stainless steel increased significantly on irradiation in oxy-

genated water but decreased slightly in the hydrogen treated water. Intergranular stress corrosion cracking was enhanced in the former case but did not occur in

the latter. These results show therefore that stress corrosion sensitivity of chromium depleted grain boundaries in stainless steel is controlled by the elec- trochemical corrosion potential established by the rele- vant radiation chemistry and electrochemistry.

A more complicated variant of the tests described above has been carried out recently in which crack propagation rates were measured in a precracked spec- imen of thermally sensitized type 304 stainless steel

Lwl. In one case [2], the irradiations were achieved using

protons of a controlled high energy produced by a cyclotron, the energy being carefully chosen to simu- late the radiolytic product concentrations typical of neutron and y radiation in a BWR. The dose to the water was therefore many times that achievable from y ray sources. Nevertheless, the results obtained on ther- mally sensitized stainless steels were qualitatively simi- lar to those obtained with y ray irradiations; i.e. a clearly defined critical cracking potential exists, above which cracking occurs. Similarly, hydrogen additions of = 150 ppb typical of modified BWR water chemistry were successful in depressing the potential below the critical cracking potential for thermally sensitized type 304 stainless steel and no stress corrosion cracking was observed. In the absence of any added hydrogen, the rate of crack growth was accelerated by the higher potentials achieved with the larger radiation dose to the water compared with conventional y ray sources. Similar observations have been made with only high intensity y rays, although in this case a rather high threshold oxygen concentration of 500 ppb was ob- served [22].

The effect of sulfate impurities and y irradiation on intergranular stress corrosion cracking in sensitized type 304 stainless steel has also been studied [22,23]. Sulfate in the absence of irradiation exacerbates crack- ing sensitivity and crack growth rates but with y irradi- ation this bad effect seems to be suppressed. However great caution should be exercised in extrapolating this observation to reactor conditions due to the lack of comparability of radiation intensity.

An important additional point to note concerning the possible influence of the core environment on stress corrosion cracking of sensitized stainless steels is that there is a general trend for the critical cracking potential to decrease with increasing temperature [18]. It has been suggested that the temperature of in-core components may be high enough to depress the critical cracking potential for sensitized stainless steel as low as the free corrosion potential in PWRs. This is specu- lation, however, and no data are available to prove or disprove it.

Page 8: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

108 P. Scott/Journal of Nuclear Materials 211 (1994) 101-122

2.4. Summary radiation chemistry

Dissolved hydrogen in PWR primary coolants is completely effective in suppressing the oxidising (and reducing) products of water radiolysis. Even the much lower concentration of hydrogen currently being evalu- ated in the modified BWR coolant chemistry is effi- cient in eliminating significant concentrations of oxy-

gen or hydrogen peroxide and in lowering corrosion potentials below the critical value for intergranular stress corrosion cracking in thermally sensitized stain- less steels.

Corrosion potentials of stainless steels and nickel base alloys exposed to strong ionising radiations in PWR primary water are deduced to be very similar to those of out-of-core components. By contrast, irradia- tion of water with no excess hydrogen causes the corrosion potentials of stainless steels to increase which enhances intergranular stress corrosion susceptibility of sensitized stainless steels (and by analogy nickel based alloys).

The only important effect of irradiation on crevices with restricted circulation of bulk water appears to be the possibility of concentrating salts by boiling induced by local y heating. In PWR primary water, this could give rise to concentrated solutions of lithium hydroxide and boric acid and undesirable corrosion side-effects.

3. Radiation damage effects

Neutron irradiation of metallic materials can lead to profound changes in mechanical and metallurgical properties of potential significance to resistance to stress corrosion cracking; those of interest here are radiation hardening, radiation enhanced creep, helium and hydrogen embrittlement and radiation induced segregation.

3.1. Hardening

One consequence of intense neutron bombardment and the creation of many vacancies, interstitials and dislocation loops is a severe hardening and loss of ductility and fracture toughness of stainless steels and nickel alloys. These phenomena have been studied extensively, most commonly at the higher temperatures of interest to Fast Reactors rather than Thermal Reac- tors. However, it is clear that the yield stress and ultimate tensile stress of stainless steels increase signif- icantly for fluences between 10” and 10z2 n/cm2 (E > 0.1 MeV) with a concomitant drastic reduction of ductility to as low as 0.3% and only a relatively small influence of composition and microstructure on the kinetics [2]. Fracture toughness is correspondingly de- creased to minimum values around 50 MPa 6 121.

At normal strain rates, tensile fractures in heavily irradiated stainless steels are nevertheless ductile transgranular, albeit of a very characteristic appear- ance due to the highly localized nature of the deforma- tion [2]. Recently, however, tensile tests on type 304 stainless steel PWR control rod cladding (described in more detail in section 4.2) have shown that the strain rate has an effect on crack morphology [6]. In fact there is an increasing tendency to substantial inter- granular fracture with decreasing strain rate between 10m5 and 10m7 s-l. Thus, slow deformation of heavily irradiated austenitic stainless steels can produce inter- granular fracture surfaces that could easily be wrongly attributed to stress corrosion cracking.

More generally, hardening to the degree implied by residual ductility as low as 0.3% would, if achieved by cold work, normally be assiduously avoided in the interests of resistance to stress corrosion. Although hardened microstructures due to irradiation and cold work may not be strictly comparable, what little data exists for aqueous environments at - 300°C indicates that 10 to 50% cold worked type 304 stainless steel does not crack in hydrogenated high temperature wa- ter but is nevertheless degraded in oxygenated water

[31. Cold work coupled with crevice geometries has also

been shown to enhance crack initiation in oxygenated high temperature water while 10% cold work has simi- larly been shown to be severely detrimental for crack propagation rates in solution annealed, type 304 stain- less steel [l]. The main risk to structural integrity in PWRs may therefore occur during refueling when the pressure vessel is open to air or, in the case of fuel elements, when exposed to the fuel cooling pond envi- ronment.

3.2. Creep

As mentioned in the Introduction, irradiation en- hanced creep may affect stress corrosion susceptibility via its influence on the applied stress. Loads may be relaxed under constant displacement loading or in- creased under non-restrained load conditions. Quanti- tative assessments are hindered by a dearth of data at typical water reactor operating temperatures but there seems to be no doubt that the effect is a significant one even at 288°C [2].

Another factor to consider is the sensitivity of stress corrosion in many passive metal/ aqueous environment systems to the applied strain rate since it controls the rupture rate of the protective oxide film. Hence a direct effect of the irradiation creep rate on stress corrosion cracking of core structural components can be anticipated [l] with a possible synergistic interaction with any helium bubble formation from transmutation reactions.

Page 9: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

P. Scott/Journal of Nuclear Materials 211 (1994) 101-122 109

3.3. Hydrogen and helium embrittlement

One possible hypothesis advanced to explain low ductility intergranular fractures observed in highly irra- diated stainless steel core components of thermal reac- tors is based on embrittlement by hydrogen and/or helium, possibly enhanced by irradiation hardening and lack of ductility of the grains themselves [24]. Both gaseous embrittlers have long been considered as a potential hazard for reactor structural materials [lo]. The principle sources of hydrogen to consider are the corrosion reactions and (n, p) nuclear reactions in the material and for helium (n, (.x) nuclear reactions.

3.3.1. Sources of hydrogen In properly controlled water chemistry, whether of

the PWR type (with hydrogen and lithium hydroxide additions) or the BWR type (pure water plus radiolyti- tally produced hydrogen and oxygen) the corrosion rate of stainless steels will be very low, say within the band 0.1 to 1.0 mg/dm’ day [11,13]. The supporting cathodic reaction is hydrogen discharge from water in totally deoxygenated PWR conditions. Even in BWR water at high temperature, the mixed corrosion poten- tial is established with a large contribution from hydro- gen evolution together with oxygen reduction [19].

Thus, a conservative estimate of the maximum cor- rosion hydrogen discharge rate assumes the maximum likely corrosion rate totally supported by hydrogen evolution; i.e. a corrosion current of 0.5 uA/cm2 which is equivalent to about 5 X lo-’ ml H2 (STP)/cm2 s. This rate of production would be enough to saturate significant thicknesses of stainless steel, 1.0 cm say, after some years although diffusion would probably be rate controlling, at least in fully austenitic steels.

Although the diffusivity and solubility of hydrogen in (unirradiated) stainless steels is well established as a function of temperature and gaseous hydrogen pres- sure [25], it is not so easy to estimate the equivalent hydrogen fugacity due to the corrosion reactions. Mea- surements of dissolved hydrogen in BWR core compo- nents have indicated values mainly between 10 and 30 wppm with a maximum of 90 wppm. There is only an apparently weak increase in concentration with neu- tron dose which suggests a small contribution from (n, p) reactions [26]. These results indicate an equivalent hydrogen fugacity of = 10 MPa at 289°C. No similar data for stainless steels have been found for PWR conditions but a similar exercise for pressure vessel steels [27] suggests hydrogen fugacities of a similar order of magnitude. Given the similar corrosion rates of stainless steel and low alloy steel in both types of water chemistry (when properly controlled) and lack of significant galvanic differences between stainless and carbon steels in each coolant, then similar limits for equivalent hydrogen fugacity can be anticipated.

The time to reach equilibrium and the extent of hydrogen homogenization in austenitic alloys depends very much on the temperature of operation, the thick- ness of components and their effects on diffusion rates

but is likely to take many years at temperatures around 300°C.

The period of equilibration could also conceivably be influenced by radiation damage since vacancy clus- ters are known to interact strongly in type 316 steels with hydrogen atoms [28]. In this study it was also noted that high energy electron predamage above 0.5 dpa produced tangled dislocations facilitating the transport of hydrogen.

Thus, overall, irradiation effects on diffusion and therefore on equilibration with the various sources of hydrogen are difficult to judge quantitatively.

3.3.2. Hydrogen embrittlement It is well documented that the ductility and UTS of

austenitic and austeno-ferritic stainless steels can be severely degraded at least at room temperature by absorbed hydrogen [29] even in the absence of irradia- tion damage. Unfortunately, studies of embrittlement often do not give details of hydrogen concentration measurements although more than 100 wppm could be expected in most cases. In fully austenitic stainless steels, severe degradation leading to cleavage type frac- ture modes has been clearly linked to the formation of (Y’ martensite by plastic deformation [1,29,30].

The martensitic deformation temperature (i.e. the temperature at which 50% of the sample transforms to martensite at 30% strain) can be used as a measure of susceptibility as defined by the empirical equation [31]:

Md(“C) = 413 - 462(C + N) - 9.2(Si) - 8.1(Mn)

- 13.7(Cr) - 9.5(Ni) - 18.5(Mo),

where the elemental concentrations are in wt%. Easily transformable stainless steels such as type

304 are much more susceptible than very stable type 310 for example. Type 316 stainless steel is also rela- tively stable with typical Md temperatures well below 0°C. The hydrogen charging process itself may also cause the formation of E martensite in the less stable steels such as type 304. Nitrogen strengthened steels show a much increased tendency to cleavage in the hydrogen charged condition [32].

Thermal sensitization of austenitic stainless steels has been observed, also in room temperature tests, to change the fracture mode of hydrogen charged speci- mens from ductile-dimple or cleavage to predomi- nantly intergranular [29,33]. Again this can be ex- plained in the case of easily transformable steels by the rise in Md temperature in the chromium depleted layer adjacent to the grain boundaries of thermally sensi- tized materials.

Page 10: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

110 P. Scott/Journal of Nuclear Materials 211 (1994) 101-122

Even types 304L and 316L stainless steels, given a sufficiently severe sensitization, can be embrittled in- tergranularly by hydrogen [33].

However, the former is more sensitive than the latter, a’ martensite being detected on the grain boundaries of strained sensitized type 304L but not of type 316L where E martensite may be present. It also seems reasonable to suppose that grain boundary im- purities such as phosphorus and sulphur and possibly nitrogen could also increase susceptibility to intergran- ular hydrogen cracking in sensitized stainless steels. As will be seen in section 3.4, chromium and molybdenum depletion together with phosphorus and sulphur en- richment are observed at the grain boundaries of heav- ily irradiated stainless steels.

Type 304L gas tungsten arc welds using a type 308L filler wire yielding _ 10% 6 ferrite have also been

tested in a high pressure hydrogen environment [34]. These tests also showed a marked reduction in ductility and change of fracture mode, in this case the fractures initiating at the y-6 interfaces. Extensive twinning and martensite platelet formation were observed which were believed to produce both high local stresses and high hydrogen concentrations at the y-6 interfaces.

The influence of increasing temperature on hydro- gen embrittlement of austenitic stainless steels is rather difficult to judge given the relative paucity of data compared to room temperature [30]. However, given the mechanistic explanation described earlier, hydro- gen embrittlement above the Md temperature would be expected to diminish rapidly at least as far as cleavage and intergranular modes of failure are con- cerned. Such an amelioration of hydrogen effects with increasing temperature has been observed, even in easily transformable steels above 100°C [30]. Reduc- tions in flow stress and ductility could nevertheless still persist at higher temperatures due to the high solubil- ity and low diffusivity of hydrogen in austenite.

It is a mute point whether irradiation induced loss of ductility (see section 2.1) could have a synergistic effect with hydrogy and enhance ductility loss or provoke intergranular cracking in types 304 and 316 stainless steels.

As noted earlier, it is known that irradiation in- duced defects act as hydrogen traps [28] and at least one easily transformable steel type 301 (cold worked) has shown increased loss of ductility in 10 MPa hydro- gen compared to an inert gas after irradiation to 1.5 X

10” n/cm2 (E > 1 MeV) t- 0.2 dpa) 1351.

3.3.3. Sources of helium The major elements and many of the minor elemen-

tal components of stainless steel and nickel base alloys undergo (n, a> nuclear reactions leading potentially to significant concentrations of helium. A comparison be- tween helium production rates from type 316 stainless

steel between thermal and fast reactors is shown in Fig. 4 [36]. Of particular note is the boron source which would very likely be segregated to grain boundaries and, if not specified, would probably be greater than the 0.003 wt% given in Fig. 4. Unlike hydrogen how- ever, helium is virtually insoluble in steels and it pre- cipitates in traps or agglomerates in bubbles. There is

x

300

n

i

THERMAL REACTOR NEUTRON FLUXES 1 .I x IO’S n.m-2 S-1 (TOTAL)

1.0 x 101a n.m-2 S-1 (WESTCOTT)

1.14 x 1017n.m-2S-1 (FISSION)

“0 500 1000

150 FAST REACTOR NEUTRON FLUXES 8.0 x 1019 n.m* S-1 (TOTAL)

1 .I x 1038 n.m2 S-1 (GROUP 1)

8.3 x 1018 n.m-2 S-1 (FISSION)

TOTAL

Y / . THRESHOLD

TIME AT POWER DAYS

Fig. 4. Helium production in type 316 stainless steel [36].

Page 11: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

P. Scott/Journal of Nuclear Materials 211 (1994) 101-122 111

therefore no thermodynamically defined upper limit on perfectly consistent with observations made more re-

concentration as in the case of hydrogen and its iso- cently in studies directly related to the phenomenon of

topes which can diffuse relatively easily to reduce local irradiation assisted stress corrosion cracking (see sec-

supersaturation. tion 3.4).

3.3.4. Helium embrittlement

Although the formation of helium bubbles both intra- and intergranularly in stainless steels is well known to cause embrittlement, loss of ductility and reduced creep strength [lo], it has not hitherto gener- ally been considered in the context of irradiation in- duced intergranular fracture at relatively low tempera- tures, e.g. < 350°C.

At higher irradiation temperatures, generally above 400°C (some authorities say 5OO”C), some migration of helium to grain boundaries and enhanced bubble for- mation can be anticipated. For example, one study of two high nickel austenitic steels irradiated to 15 dpa (in EBR II) at 625°C indicated approximately a lo3 in- crease in the grain boundary helium concentration compared to the average concentration of 15 appm [37]. This was sufficient to cause intergranular cracking in room temperature tensile tests in vacuum.

In another study of the influence of irradiation temperature and tensile test temperature on the ten- sile properties of type 347 and 348 stainless steels, conclusive evidence of the involvement of helium em- brittlement after irradiations to 4.4 x lO*l n/cm’ (E > 1 MeV) t N 6 dpa) was only obtained at fracture test temperatures above 500°C but less than 650°C [41]. The helium concentration measured for the highest neutron dose was 37 appm which was more than dou- ble that calculated from the fast neutron dose alone.

Similarly, in an examination of the weldability of solution annealed and 20% cold worked type 316 stain- less steel with helium implanted through tritium decay, as little as 2.5 appm helium was sufficient to cause severe heat affected zone cracking [38]. In this case, the position of the crack corresponded to a maximum temperature in the heating cycle of 1150°C. By con- trast, stainless steels irradiated at less than 400°C and tested at less than 400°C even with very high concen- trations of helium did not show any serious losses of ductility in conventional tensile tests [39].

The decay of implanted tritium in stainless steels to helium has been used to assess the effects of helium embrittlement independent of radiation damage. Con- centrations of 30 appm He3 introduced at 200°C were found not to affect significantly the ductility of types 304L and 309s stainless steels in room temperature tensile tests at normal strain rates whereas in tests at 700°C severe intergranular embrittlement was observed [42]. Nevertheless, at low temperatures, fairly evenly distributed bubbles of helium of about 4.5 nm diameter were observed which gave rise to some increase in the measured yield strengths.

The lowest temperature irradiation known to give rise conclusively to helium bubble embrittlement of grain boundaries, in this case of type 304 stainless steel, was at 370°C [40].The fast neutron dose was between 1.4 X 10” (- 7 dpa) and 1O23 n/cm* (E > 0.1 MeV) (_ 50 dpa) and the helium content 28 appm for the highest dose. The specimens were fractured in this work at 550°C in an Auger spectrometer without any reported attempt to control the strain rate. Very low ductility intergranular fractures were usually obtained, the exceptions being some examples of ductile be- haviour at the lowest dose.

In a similar study of hydrogen isotope and helium embrittlement of types 304L, 309S, 304LW and 316L stainless steels [43], all three isotopes of hydrogen produced similar effects on mechanical behaviour at room temperature to those described in section 3.3.2. If the tritium was allowed sufficient time to decay to 30 or 50 appm He3 followed by vacuum removal of resid- ual tritium, ductility losses and intergranular fracture were again only observed after high temperature an- neals which allowed helium bubbles to agglomerate on the grain boundaries.

Reference was also made by these authors [40] to low ductility intergranular “creep-rupture” fractures observed in other work at 450, 550 and 600°C test temperatures. A volume extending about 300 nm either side of the grain boundary contributed to helium re- lease during intergranular fracture at 550°C suggesting that only 4.5% of the boundary surfaces on average was covered with helium bubbles. Additionally, the redistribution of major and minor elements observed by Auger spectroscopy at the grain boundaries were

Helium concentrations in excess of 200 appm have also been observed to cause ductility losses at normal strain rates in type 304L stainless steel and welds at room temperature but by enhancing microvoid coales- cence and not along ‘Y’-y or 6-y boundaries as with hydrogen embrittlement. A 21Cr, 6Ni, 9Mn alloy with a similar helium content failed intergranularly at room temperature in the same study whereas the corre- sponding weld metal 22Cr13Ni5Mn failed by microvoid coalescence.

In summary, helium effects on the fracture of stain- less steel are in general more severe than hydrogen effects at similar concentrations and particularly so if sufficient helium bubbles form on grain boundaries to provoke intergranular failure. The predicted helium production rate given in Fig. 4 could in principle be sufficient to cause problem after a few reactor cycles.

The risk would be enhanced if boron was segre- gated at grain boundaries or if the temperature was

Page 12: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

112 P. Scott /Journal of Nuclear Materials 211 (1994) 101-122

high enough, even transiently, to permit diffusion of helium to grain boundaries. The effect of operating temperature maintained below 500°C is very difficult to quantity precisely on the basis of current data, al- though the risk of helium agglomeration on grain boundaries seems slight at normal reactor operating temperatures.

3.4. Segregation

A detailed review of this important phenomenon for IASCC has been made by Andresen et al. [1,2] and so only the main points are reiterated here.

Fast neutron irradiation of metallic alloys causes atoms to be displaced from their normal lattice posi- tions thus generating vacancy and interstitial point defects. Many of these recombine but at temperatures of interest to LWRs (and indeed other thermal reac- tors) some of these point defects migrate relatively long distances to natural sinks such as surfaces, dislo- cations and grain boundaries. This process leads to a redistribution of alloying elements near these sinks since different elements diffuse at different rates. Some elements such as Si, P and possibly nickel are believed to migrate mainly by interstitial mechanisms and are enriched near sinks while other solutes such as chromium, iron and molybdenum exchange more rapidly with vacancies and are consequently depleted near vacancy sinks. The competition between point defect generation during neutron irradiation and re- combination gives rise to a temperature/dose rate dependence of the conditions under which segregation

RADIATION-INDUCED SEGREGATION

933

761

589

72

-101

10-e 16’ 1o.O 1C 16' 12

RADIATION FLUX, dpa i s

Fig. 5. Temperature/flux diagram showing the band in which radiation induced segregation is most pronounced [1,2].

DISTANCE (mm)

Fig. 6. Compositional profiles by dedicated STEM analysis

across grain boundaries from a type HP348 stainless steel

irradiated to 3.4~ lo’* n/cm2 in a BWR [44].

is likely to occur; Fig. 5 [1,2]. Such processes are absolutely fundamental and cannot be avoided al- though the kinetics may be influenced by metallurgical factors.

The experimental evidence for these mechanisms of radiation induced segregation is now strongly estab- lished. The magnitude of segregation or desegregation at grain boundaries can be substantial as illustrated in Fig. 6 for a type 348 stainless steel irradiated to 1 or 2 dpa in an LWR [44]. Qualitatively, similar profiles of segregated/desegregated species have been observed in types 304, 316, 348 and 20% Cr/20% Ni/Nb stain- less steel irradiated at u 300°C [1,2,40,44-471 and in other stainless steels and nickel alloys irradiated at higher temperatures [48,49]. Thus at 3OO”C, chromium and iron are typically depleted by 5 to 10 wt% from the bulk concentration in type 3xx stainless steels, even in Nb stabilized types, whereas nickel is enriched by about 5 to 10 wt% from the bulk concentration, Fig. 7 [44].

Page 13: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

P. Scott/Journal of Nuclear Materials 211 (1994) 101-122

Radiation Induced Segregation Dedicated STEM Data of Jacobs & Sheperds

CP348 BWR 1.5~10~’ n/cm2 HP348 BWA 3.4~10~’ n/cm2

113

Cr

Fig. 7. Comparison of dedicated STEM analysis data from commercial purity and high purity type 348 stainless steel irradiated to

various fluences in a BWR [44].

Radiation Induced Segregation Auger Data of Jacobs & Clausing Data normalized to Fe + Ni + Cr peak Ratio = (IG data) I (ductile data)

Fig. 8. Comparison of Auger spectroscopy data from commercial purity types 304 and 348 and high purity type 348 stainless steels irradiated to various fluences in an advanced test reactor or BWR [44].

Page 14: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

114 P. Scott /Journal of Nuclear Materials 211 (1994) 101-122

Molybdenum is also depleted but to a lesser extent of = 2% [47]. Silicon is observed to be significantly enriched by three to five times the bulk concentration [44,45,47] even to the extent of forming Ni,Si precipi- tates in stainless steels with a somewhat higher nickel content than typical of the type 3xx series 1491.

The common impurity elements sulphur and phos- phorus tend to be enriched at grain boundaries al- though the data can be rather scattered; Fig. 8 [44]. The dose dependence of segregation is illustrated in Fig. 9 [47] from which it is seen that segregation is readily detectable for doses above 102’ n/cm2 (E > 1 MeV).

Extremely narrow segregation profiles (< 10 nm) are observed for irradiations at = 300°C (Fig. 7). At higher temperatures, the magnitude of the segregation at grain boundaries is reduced and the widths of the zones affected are increased. Various synergistic ef- fects between different elements are also known or suspected as having an influence on segregation. Nev- ertheless, good quantitative agreement has been achieved between experiment and theoretical mod- elling of irradiation induced segregation of certain elements, notably Fe, Ni, Cr, by the inverse Kirkendal mechanism [1,49]. At LWR temperatures, significant segregation is predicted at a dose of 0.1 dpa and saturation of the effect at about 10 dpa. Some progress is also being made in modelling phosphorus, sulphur and silicon segregation by interstitial mechanisms [1,.50].

The extreme narrowness of the segregated zones at grain boundaries in stainless steels irradiated at LWR temperatures creates very great technical difficulties for quantitative characterization, to say nothing of the added complexity of working with activated alloys emit- ting high energy y rays. Most success has been achieved using high resolution scanning electron microscopy with an exceedingly high brightness field emission electron gun and a beam diameter of = 2 nm [44-471. Conven- tional instruments with typically 10 to 20 nm diameter electron beams are unable to detect segregation on the required scale. In addition, special equipment and great care and skill are required in the preparation of the specimen foils and in the analysis of the X-ray spectra which are complicated by background y ray emissions from the specimen. Auger spectroscopy can also be effective on the necessary geometric scale, particularly for sulphur and phosphorus, provided intergranular cracking can be provoked in the spectrometer and the JJ radiation can be tolerated from the relatively large specimens usually employed [40,51]. Martensitic trans- formations can complicate specimen preparation for Auger or STEM studies in type 304 stainless steels, particularly high purity casts.

Hydrogen embritttement used to encourage inter- granular fracture in Auger spectrometers may also reveal the importance of different elements to those

o:sus304

q :SUS316 -10

~~

P

’ “““” ’ “““” “ +4 1

+2C fp

-6

4 110 a 3

.;*24 102s 1026

Neutron fluence (n/m% E > 1 Mev) Fig. 9. Neutron fluence dependence of grain boundary segre- gation in types 304 and 316 stainless steel 1471.

which are significant in high temperature water. Atom probe techniques can also be applicable provided again that the background radiation can be tolerated and that a grain boundary can be located sufficiently close to the tip of the probe.

Page 15: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

P. Scott /Journal of Nuclear Materials 211 (1994) 101-122 11.5

3.5. Stress corrosion cracking 3.5.2. Stress corrosion cracking tests

What then are the implications of irradiation in- duced segregation for stress corrosion resistance in PWR and BWR environments or indeed for standard chemical or electrochemical tests for grain boundary segregation? We include in this section all known data concerning postirradiation tests. Results from experi- ments in reactor cores are included in the next section

on in-reactor experience.

3.5.1. Grain boundary segregation tests Of the common tests used to detect grain boundary

chromium depletion [52,53], the Strauss test has been shown to be ineffective in stainless steels irradiated to 1 or 2 dpa which have nevertheless cracked in service in oxygenated aqueous environments at N 300°C [1,49]. The width of the zone of chromium depletion of < 13.2% appears to be a crucial parameter controlling the efficacy of these tests.

From the analysis of component failures in BWRs and slow strain rate tests on preirradiated type 304 and 316 stainless steels in simulated BWR water (at 288”C), a threshold dose of 5 X lo*’ n/cm* (E > 1 MeV) (- 1 dpa) for the onset of IASCC has been deduced [1,2,44,46,56,57,15,58,59]. This threshold has been widely attributed to the development of chromium depleted grain boundaries as described in section 3.4. Moreover, typical dependence of intergranular stress corrosion cracking of sensitized stainless steels on oxy- gen concentration is observed. Thus, intergranular cracking can be suppressed in deoxygenated solutions at least for the lower neutron doses (5 X lo*’ to 2 X lO*i n/cm2 E > 1 MeV).

In LWR irradiated materials this zone is less than about 6 nm wide and is ten times narrower than typical of thermally sensitized materials. A chromium de- pleted width of 6 nm was found to be the minimum width necessary for the Strauss test to respond follow- ing irradiation over a range of higher temperatures [49]. The EPR test would be expected to have a rather similar response to the Strauss test and has successfully detected chromium depletion induced by irradiation at 420°C [54]. However, there could be electrochemical complications on specimens with high y activities.

A quantitative relationship between neutron dose above 5 x lo*’ n/cm2 (E > 1 MeV) (- 1 dpa), mea- sured grain boundary chromium depletion and IGSCC (IASCC) susceptibility has proved elusive however [60]. Indeed, it is now clear that for type 316 steel irradiated to a neutron dose of 9 X 10” n/cm* (E > 1 MeV) (_ 13 dpa), intergranular cracking cannot be com- pletely prevented by reducing the oxygen concentration in water at 288°C to values consistent with corrosion potentials less than the critical cracking potential for thermally sensitized stainless steels.

Boiling nitric acid tests which are also sensitive to phosphorus and silicon segregation have also been used to characterize irradiated stainless steels [55]. The degree of grain boundary dissolution does appear to vary continuously with fast neutron dose and some correlation with PWR and BWR plant failures has been observed [ 1,2,4,44,56,57].

Observations that some type 304 and 316 stainless steel PWR components exhibit a minimum fast neu- tron dose threshold of c 2 x 10” n/cm* (E > 1 MeV) (- 3 dpa for intergranular cracking (section 4.2) rein- force the idea that another cracking mechanism oper- ates in the higher dose regimes which is not related to grain boundary chromium depletion) [1,26,8,9].

Nevertheless, their sensitivity to phosphorus segre- gation in particular, for which there is no satisfactory evidence of it being important to stress corrosion in high temperature water reactor environments and good electrochemical arguments why it may not be impor- tant [l], suggests again that such results could be misleading.

In addition, relatively recent in-reactor experiments (section 4.1) on several different stainless steels using a swelling capsule technique gave generally very low di- ametral strains to failure (with the exception of one ultra pure heat of type 348 stainless steel) whether exposed to BWR or PWR water [61]. In fact, in both water chemistry types the apparent threshold fast neu- tron dose for cracking in these experiments was much closer to that believed to be characteristic of PWRs.

An alternative deduction could be (see later) that the failure mechanism of some in plant components, particularly at high neutron doses > lO*l n/cm* (E > 1 MeV) is not stress corrosion but that these nitric acid tests reveal the microstructural changes responsible for whatever intergranular cracking mechanism is relevant.

It is concluded that the results of all low tempera- ture diagnostic tests for grain boundary segregation in irradiated stainless steels (or nickel alloys) must be treated with great caution. They can be ineffective and/or misleading.

We conclude therefore that irradiation induced grain boundary depletion of chromium can explain some observed cases of intergranular cracking particu- larly in oxygenated BWR environments and for neu- tron doses between about 5 X lo*’ (- 1 dpa) and 2 x lO*l n/cm2 (E > 1 MeV) ( _ 3 dpa). However, it does not explain the higher dose failures and those occur- ring in totally deoxygenated PWR environments where corrosion potentials are well below the critical cracking potential for sensitized stainless steels. It now seems clear that one or more of the embrittlement mecha- nisms discussed earlier probably play a role.

While the role played by neutron irradiation in- duced grain boundary chromium depletion in the

Page 16: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

116 P. Scott/Journal of Nuclear Materials 211 (1994) 101-122

IASCC of stainless steels in oxygenated water is rea- sonably clear, the role of other segregated/desegre- gated elements is much less clear. Their significance can only be assessed from some knowledge of their electrochemical characteristics and effects in other nonirradiated stress corrosion studies.

No particular significance in either BWR or PWR environments has so far been attributed to irradiation induced nickel enrichment or iron and molybdenum depletion at grain boundaries in stainless steels. How- ever, martensitic transformations could in principle be facilitated in the grain boundary zones possibly encour- aging sensitivity to hydrogen embrittlement at rela- tively low temperature (during plant shutdown for ex- ample). An intriguing question for PWRs is whether, after prolonged neutron irradiation, the grain bound- aries could resemble those of a nickel base alloy such as alloy 600. However, the magnitudes of segregation/ desegregation observed in type 3xx stainless steels, even at relatively high neutron doses, does not suggest that this is a realistic possibility.

Of the minor alloying or impurity elements, con- cerns have been mainly focussed on silicon, phospho- rus and sulphur segregation although this often ap- pears to be an instinctive reaction rather than derived from hard evidence other than via the doubtful means of the boiling nitric acid test [6,57]. Recent work on irradiated model alloys seems to confirm this opinion for BWR conditions [46,62].

Nevertheless, silicon and phosphorus specifications have recently been reduced significantly for LWR con- trol rod cladding. The only known evidence for their possible significance comes from observed improve- ments in the resistance of stainless steel fuel cladding to intergranular cracking in the early years of LWR fuel development [l-4] and the in-reactor swelling capsules experiments [61]. From a basic electrochemi- cal view point, it is difficult to see why phosphorus should be important in either BWR or PWR environ- ments; it requires higher potentials as in nitric acid to dissolve. However, phosphorus could be important in other types of intergranular embrittlement.

Silicon on the other hand is highly surface active and any tendency to form silica based oxide films over grain boundaries enriched in silicon would seem to be undesirable since silica readily dissolves in high tem- perature water, (independent of water chemistry in the range of interest). Recent work appears to discount this possibility, however [46,62].

Sulphur segregation to grain boundaries in irradi- ated stainless steels is not consistently observed but is believed to act synergistically with chromium depletion in typical BWR normal water chemistry conditions [l]. Nitrogen, carbon and boron are other minor elements which could be significant for intergranular cracking susceptibility through their influence on irradiation

damage. Boron has already been discussed in the con- text of helium generation.

Finally, it is necessary to add a caution that general conclusions concerning grain boundary segregation in stainless steels and effects on stress corrosion suscepti- bility should not be assumed to apply to nickel base alloys. The relatively poor performance of alloy 600 in PWR primary water with regard to intergranular stress corrosion cracking and also with analogous higher strength alloys in the absence of irradiation suggests a different mechanism of cracking to that relevant to stainless steels. Information on irradiated nickel alloys is very sparse and it is extremely difficult to draw any conclusions or general trends from the data available for light water reactor coolants.

3.6. Summary

Radiation induced segregation or desegregation of elements at grain boundaries in neutron irradiated stainless steels or nickel base alloys is generally ac- cepted to be an important precursor of irradiation assisted stress corrosion cracking. The process is abso- lutely fundamental to materials exposed to fast neu- trons and becomes detectable at doses of 0.1 dpa, significant at doses of 1.0 dpa and saturates at about 10 dpa. The zones affected adjacent to grain boundaries are typically very narrow, < 10 nm wide, in materials irradiated at water reactor core temperatures, and are difficult to characterise experimentally.

Radiation hardening and radiation induced creep may also be important contributory factors to stress corrosion sensitivity.

Since radiation damage induced processes are com- mon to irradiated components of all types of nuclear reactor, the difference between the apparent threshold neutron doses for cracking for BWRs and PWRs illus- trates the importance of the synergistic interactions with the relevant environmental chemistry.

Grain boundary chromium depletion in stainless steels appears to be the main factor controlling IASCC sensitivity in BWR environments but is not important in PWR environments. Helium and hydrogen produc- tion by neutron capture reactions are also of concern because of the embrittlement they cause. There is a high probability of intergranular failure if an alloy containing intragranular helium is heated for whatever reason above - 450 to 500°C due to diffusion and bubble formation on grain boundaries.

4. In-reactor experience

The discussion here is divided into two parts; the first dealing with in-core reactor experiments and the

Page 17: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

P. Scott /Journal of Nuclear Materials 211 (1994) 101-122 111

second with known component failures and their diag- nosis.

4.1. Reactor experiments

Two important series of in-reactor experiments have been conducted in recent years in order to try and understand the critical parameters and to identify al- loys showing better resistance to IASCC. Notably, both have been carried out in power reactors and not test reactors.

The first set of experiments has exclusively con- cerned BWRs [1,2]. Various self-loaded, precracked specimens of type 304 stainless steel were exposed in the high flux region of the Nine Mile Point no. 1 BWR and the crack length was monitored continuously with time. Crack growth occurred virtually immediately in the case of thermally sensitized material but a signifi- cant incubation period was noted in the case of solu- tion annealed materials. These results were consistent with the assumption of a threshold fast neutron dose for BWRs of = 5 X 102’ n/cm2 (3 1 dpa). The rates

of crack growth observed were faster than those mea- sured in the absence of irradiation. They were also consistent with the predictions of a theoretical model based on anodic dissolution of chromium depleted grain boundaries at electrochemical potentials con- trolled by realistically estimated core concentrations of oxygen and hydrogen peroxide. It is not obvious, how- ever, that these remarkably successful results and model predictions are applicable to PWR water chemistry, since anodic dissolution cannot necessarily be pre- sumed to be a relevant mechanism in the latter case.

The second set of experiments have compared both BWR and PWR systems by utilizing a capsule test method in which a mixture of alumina and boron

DIN 1.4541

a b c

carbide swells slowly during irradiation [61]. By using different proportions of alumina and boron carbide, the strain rate applied to the capsule wall was varied. The exterior surfaces of the capsules were exposed to the relevant reactor coolant in a fuel element position. Fig. 10 shows the results obtained in the PWR after two reactor cycles for various stainless steels and nickel alloys. In general, the results obtained in terms of diametral strain to failure were not that different from those obtained in the BWR.

Both the type 321 stainless steel and the Inconel 718 were somewhat worse in the PWR environment although the latter when correctly heat treated also did quite well. Only a high purity heat of type 348 stainless steel (S 0.007%, P 0.002%, Si 0.02% compared to S 0.009%, P 0.009% and Si 0.34% in the commercial heat) performed well in both environments. Weight loss measurements on the stainless steels in the Huey test after irradiation were also much lower in the high purity type 348 heat. This was attributed to the low alloy concentrations of Si, P and N although only the silicon content seemed markedly different from the

comparable commercial heat of type 348 stainless steel. Nevertheless, subsequent experiments on different hight purity heats have failed to reproduce this favourable result [63].

In the case of the more numerous type 321 stainless steel capsules, the results were analysed in terms of the increase in diametral strain and fast neutron fluence, Fig. 11 [61]. At the lowest swelling rate, the yield strength (corrected for radiation embrittlement) was never exceeded. At higher swelling rates, it can be seen that a minimum diametral failure strain of - 0.8% (equivalent to - 2.5% elongation) was observed at a dose of - 1021 n/cm2 (E > 1 MeV). Comparing BWR and PWR water environments, it was observed that the latter was slightly worse.

AlSl AIS 348 INC 625 INC X 750 INC 718

316 a b a b a b c a b

Fig. 10. Strain to failure of various alloys in the core of a PWR after 1 or 2 cycles [61].

Page 18: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

118 P. Scott /Journal of Nuclear Materials 211 (1994) 101-122

1.5 , -

I

Fatied Non -i&d

l 0 BWR m 0 PWR

Fig. 11. Map of the range of failures of DIN 1.4541 (type 321)

stainless steel samples as a function of average diameter change and fast neutron fluence [61].

This critical dose of - 10zl n/cm2 (E > 1 MeV)

corresponds to that derived from stainless steel fuel and control rod cladding in PWRs (see later) whereas IASCC in BWRs has been associated with a lower dose threshold of 5 x 10" n/cm2 (E > 1 MeV) [l--S]. Thus the slightly worse performance indicated in the capsule tests for PWR conditions (Fig. 11) is, at first sight, at variance with practical experience. However, it is re- called that there are strong indications from postirradi- ation slow strain rate tests in normal BWR water chemistry and the hydrogen dosed variant for BWRs of two separate failure processes; one due to chromium depletion at doses around 5 x 102’ n/cm2 (E > 1 MeVI and a second at higher doses, By implication, the second occurring at doses on the order of 2 X 1021 n/cm2 (E > 1 MeV), which cannot be controlled by hydrogen additions, is also relevant to PWRs. It is suggested that this second higher dose mechanism is unrelated to localised dissolution of irradiation in- duced chromium depleted grain boundaries and was the cause of cracking in the swelling capsule tests. It is noteworthy that the original authors [61] concluded that radiation creep probably contributed to stress relaxation at higher doses thus leading to the ductility minimum seen in Fig. 11. In the next subsection, we shall see that intergranular cracking can be observed in heavily irradiated stainless steels when subjected to

slow strain rate tests in the absence of any aqueous corrosion 16,641.

It is also recalled that cold worked (hardened} stain- less steels are not apparently sensitive to intergranular cracking in hydrogenated water at 300°C [3].

It is concluded, therefore, that there is a strong possibility that the failure mechanism observed in the capsme tests on stainless steels at a high dose of - 10” n/cm’ (E > 3 MeV) was mainly due to intrin- sic radiation damage with a possible involvement of hydrogen/ helium embrittlement.

For the capsule tests on nickel base alloys Inconel 625, X 7.50 and 718, no dose dependency of the failure strain was observed between 5 x lo*’ and 4 x lO*l n/cm’. The calculated diametral failure stress for In- cone1 X 750 was found, however, to be somewhat reduced compared to comparable data without irradia- tion. (In this case, the age hardened condition tested was already susceptible to intergranular stress corro- sion cracking in LWR environments in the absence of irradiation).

4.2. Power reactor experience

The earliest experience of cracking in stainless steels attributed to irradiation effects occurred during the development of fuel ctadding until zirconium alloys for this purpose reduced interest in stainless steels [l-4]. Such cladding failures occurred predominantly in BWRs although a few were also observed in PWR fuel elements. The cracks apparently initiated on the exter- nal surface and showed a clear dependence on neutron flux and cladding strains generated by fuel pellet sweliing. Postirradiation tests, presumably at relatively high strain rates, showed only ductile rupture. At that time, the BWR incidents were associated with an ap- parent threshold fast neutron dose of = 5 x 102” n/cm2 while the PWR incidents were attributed to periods of poor water chemistry. Later, an apparent threshold of = 10” n/cm* was calculated [1,2,5,7]. In retrospect, the attribution to poor PWR primary water chemistry appears suspect and the threshold dose may better be associated with radiation damage mecha- nisms.

Intergranular cracking of other irradiated stainless steel components listed in Table 1 in BWR or other oxygenated environments have been broadly consistent with the threshold neutron doses of 5 X 102” n/cm2 (E > 1 MeV) identified above [1,2]. For stainless steel components in PWRs, the picture is more complicated. For example, failures of instrument dry tubes in PWRs have been attributed to flow induced vibration and wear.

A similar wear problem has also affected control rod cladding integrity but in this case cracking has also been observed [6,8,64]. As in the case of fuel cladding,

Page 19: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

P. Scott/Journal of Nuclear Materials 211 (1994) 101-122 119

0.1 /

-12 -10 -8 -6 -4 -2 0 2

Log (E I / set)

Fig. 12. Irradiated cladding tensile test results; percentage intergranular fracture versus strain rate; test temperature 600”F, argon atmosphere [64].

strains are imposed by swelling of the pin contents during neutron irradiation and consequent pellet/clad interactions. It is also not clear from evidence currently available from destructive examination whether cracks initiated from the interior or exterior of the control rod cladding.

In laboratory tensile tests in argon at 288°C how- ever, significant intergranular cracking was observed at low strain rates of - lo-’ s-l but not a high strain rates of - 10W5 s-‘, Fig. 12 1641. The cracking initiated from the original internal surface but was attributed by the authors to a mechanical effect due to the curvature of the tensile specimen machined from the original cladding. There is also a possibility that products of neutron capture reactions with the absorber elements could influence cracking from the internal surface. The only likely one from the silver-indium-cadmium ab- sorber would appear to be tin arising from the neu- tron-indium reaction. It is equally possible that the cracking is simply mechanical due to high strains ap- plied to material with very low ductility following ex- tensive neutron irradiation.

Recent examinations of failed type 316 stainless steel bolts in the core baffle assembly of some 900 MWe French PWRs have revealed intergranular frac-

ture surfaces [9] and IASCC has been considered as a possible cause. It is noted that the bolts which cracked were found in confined crevice zones subject to signifi- cant heating and strain cycles up to 0.5% during the heat up/cool down transient. However, if fatigue was the principal failure mechanism, then a transgranular fracture surface would be expected unless there was some serious weakening of the grain boundaries by radiation creep, hydrogen emb~ttlement or helium bubble formation for example. In this case, slow strain fatigue cycles could interact adversely with such inter- granular damage processes (i.e. creep-fatigue) and con- ceivably produce an intergranular fracture surface. The imposition of a slow strain rate would in any case be expected from the earlier results on control rod cladding to increase the intergranular component of failure without the intervention necessarily of corro- sion. Alternatively heating of the crevice containing the bolt could concentrate the lithium hydroxide and boric acid with potentially serious consequences for stress corrosion cracking.

Intergranular stress corrosion cracking in high strength precipitation hardened alloys such as A-286 stainless steel and Inconel X 750 has been observed frequently in the absence of irradiation. Irradiation effects are not likely to have been significant in most cases. This is particularly the case with Inconel X 750 control rod guide tube support pins where the end-of- design life fast neutron dose is anticipated to be only 5 X 102’ n/cm2 (E > 1 MeV). Therefore, since failures have been observed after only a few years, it seems unlikely that radiation damage and IASCC are contrib- utory factors. However, as heat treatments and other design improvements have now enormously improved the out-of-reactor stress corrosion resistance in PWR primary water, some care must be taken with any cases where the radiation damage may be significant over a longer period of time. In addition, any non-standard water chemistry which may be associated with closed crevices must be considered.

4.3. Summary

Stainless steel and possibly nickel alloy core compo- nent failures in BWRs are associated with a threshold neutron dose of 5 X 10” n/cm’ (E > 1 MeV) whereas a higher threshold of N 2 x 10” n/cm2 (E > 1 MeV) is typical of PWRs. In the case of BWRs, radiation induced grain boundary segregation associated with such neutron dose levels, particularly chromium deple- tion, and the electrochemical effects of ionising radia- tions on the water environment appear to explain the observed component failures. Practical solutions for BWRs are therefore directed at ameliorating these processes by hydrogen additions to the coolant as well as reducing service stresses or strains.

Page 20: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

120 P. Scott /Journal of Nuclear Materials 211 (1994) 101-122

At the higher dose of - 2 x 1021 n/cm2, a second mechanism of failure appears to be important which cannot be ameliorated by hydrogen additions to the environment. This mechanism may be common to both BWRs and PWRs. On present evidence, corrosion effects do not seem to be crucial and a radiation damage process may explain the observations, possibly with the involvement of hydrogen or helium embrittle- ment.

High strength alloys such as A 286 stainless steel and Inconel X 750 have been found to be susceptible to intergranular stress corrosion in the absence of irradiation in both BWR and PWR systems. It is diffi- cult to determine whether any additional effect of irradiation contributed to the failures of these high strength alloys but on present evidence this seems unlikely.

5. Conclusions

Dissolved hydrogen in PWR primary water sup- presses completely water radiolysis thus preventing any net change in composition and consequently any change in corrosion or redox potentials compared to those of similar materials out-of-core. By contrast, the produc- tion of oxygen and particularly metastable hydrogen peroxide in BWR cores results in anodic polarisation by up to +250 mV (SHE) compared to out-of-core components.

Fast neutron damage to stainless steels (and nickel alloys) induces significant microstructural changes in- cluding hardening, creep, helium embrittlement and grain boundary segregation/desegregation. The last.of these is generally cited as the main cause of IASCC after certain neutron dose thresholds - 5 X 102” n/cm2 (E > 1 MeV) or approximately 1.0 dpa for BWRs and - 2 x 1021 (E > 1 MeV) or approximately 4 dpa for PWRs. However, there is presently no strong evidence for irradiation effects on cracking of nickel alloy components in PWRs which are located in rela- tively low irradiation dose zones.

The lower dose threshold for BWRs appears to be associated with grain boundary chromium depletion and can be ameliorated by additions of hydrogen to the

coolant, It is therefore not significant for PWR primary circuit components. Other grain boundary segregants such as phosphorus and silicon enrichment could be significant for both reactor types but there is no hard evidence.

The higher dose threshold for intergranular crack- ing formerly associated only with PWRs also appears in the hydrogen modified BWR water chemistry. It is not obvious that corrosion plays a dominant role in this failure process. Irradiation damage could be sufficient to explain present observations possibly associated with

hydrogen or helium embrittlement. The latter may be particularly important if the temperature rises, for whatever reason, above - 450 to 500°C.

References

[l] P.L. Andresen, F.P. Ford, S.M. Murphy and J.M. Perks, Proc. 4th Int. Conf. on Environmental Degradation of Materials in Nuclear Power Systems - Water Reactors,

Jekyll Island, GA, August 1989 (NACE, Houston, 1990)

p. l-83.

[2] P.L. Andresen, in Stress Corrosion Cracking - Material

Performance and Evaluation, ed. R.H. Jones (ASM, 1992)

p. 181.

[3] R.H. Cowan and G.M. Gordon, Proc. Stress Corrosion

Cracking and Hydrogen Embrittlement of Iron Base Al-

loys, Unieux-Firminy, France, June 12-16, 1973 (NACE,

Houston, 1977) p. 1023.

[4] F. Garzarolli, H. Rubel and E. Steinberg, Proc. 1st Int.

Symp. on Environmental Degradation of Materials in

Nuclear Power Systems - Water Reactors, Myrtle Beach,

August 22-25, 1983 (NACE, Houston, 1984) p. 1.

[5] H. Hanninen and I. Aho-Mantila, Proc. 3rd Int. Symp. on

Environmental Degradation of Materials in Nuclear

Power Systems - Water Reactors, Traverse City, Michi-

gan, August 30-September 3, 1987 (AIME, Warrendale,

Pennsylvania, 1988) p. 77.

[6] M.P. Manahan, R. Kohli, J. Santucci and P. Sipush, Nucl.

Eng. Des. 113 (1989) 297.

[7] K. Pettersson (ed.), Regulatory and Life Limiting Aspects

of Core Internals and Pressure Vessels, CSNI Report no.

146 (1988).

[8] F. Cattant, C. Lebuffe, J. Dechelotte, A. Raybaud and

M. Ladouceur, Proc. Int. Symp., Fontevraud II, lo-14

September 1990, Socit% Franqaise d’Energie Nucltaire,

Paris (1990) p. 151.

[9] Ph. Berge and F. De Keroulas, Proc. 4th Int. Conf. on

Environmental Degradation of Materials in Nuclear

Power Systems - Water Reactors, Jekyll Island, GA,

August 1989 (NACE, Houston, 1990) p. l-11.

[lo] J.L. Boutard, J. Nucl. Mater. 174 (1990) 240. [ll] P. Cohen, Water Coolant Technology of Power Reactors

CANS, 1980).

[12] W.G. Burns and P.B. Moore, Radiat. Eff. 30 (1976) 233.

[13] Y. Solomon, Proc. Water Chemistry of Nuclear Reactor

Systems, Bournemouth, 24-27/10/78 (BNES, London,

1979) p. 101.

(141 C.P. Ruiz, C.C. Him, T.L. Wang, R.N. Robinson and

R.J. Law, Modelling hydrogen water chemistry for BWR applications, EPRI Report NP 6386 (1989).

[15] M.E. Indig, J.L. Nelson and G.P. Wozadlo, Proc. 5th Int.

Symp. on Environmental Degradation of Materials in

Nuclear Power Systems - Water Reactors, 25-29 August 1991, Monterey, California, p. 941 CANS, La Grange

Park, IL, 1992).

[16] M.E. Indig, Proc. 4th Int. Symp. on Environmental

Degradation of Materials in Nuclear Power Systems -

Water Reactors, Jekyll Island, GA, August 1989, p. 4.111

(NACE, Houston, 1990).

Page 21: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

P. Scott /Journal of Nuclear Materials 21 I (1994) 101-122 121

[17] M.E. Indig and J.L. Nelson, Corrosion 47 (19911 202.

[18] P.L. Airey, Radiat. Res. Rev. 5 (19731 341.

[19] D.D. MacDonald, Proc. 5th Int. Symp. on Environmental Degradation of Materials in Nuclear Power Systems -

Water Reactors, Monterey, California, August 25-29,

1991 CANS, La Grange Park, IL, 1992).

[20] N. Fujita, M. Akiyama and T. Tamura, Corrosion 37

(1981) 335.

[21] A. Sudo, M. Itow, T. Okada, N. Saito, N. Ichikawa and Y. Hemmi, Proc. 1988 JAIF Int. Conf. on Water Chem-

istry in Nuclear Power Plants - Operational Experience

and New Technologies for Management, April 1988, vol.

2 (Japan Atomic Industrial Forum, Tokyo, 1988) p. 19.

[22] K. Nakata, S. Shimanuki, H. Anzai, K. Mabuchi, M. Fuse

and N. Shigenaka, Proc. 5th Int. Symp. on Environmental

Degradation of Materials in Nuclear Power Systems -

Water Reactors, 25-29 August 1991, Monterey, CA

CANS, La Grange Park, IL, 1992) p. 955.

[23] N. Saito, N. Ichikawa, Y. Hemmi, A. Sudo, M. Itow and

T. Okado, Corrosion 46 (1990) 531.

[24] H. Hanninen and I. Aho-Mantila, Proc. Environmental

Degradation of Materials in Nuclear Power Systems -

Water Reactors, Traverse City, Michigan, August 30-

September 3, 1987 (AIME, Warrendale, Pennsylvania,

1988) p. 77.

[25] D.R. Harries, Radiat. Eff. 101 (1986) 3.

[26] A.J. Jacobs, Hydrogen buildup in irradiated Type 304 stainless steel, in ASTM STP 956 Influence of Radiation

on Material Properties, 13th Int. Symp., Seatle, Washing-

ton, 23-25 June 1986 (Part II) (1987) p. 239.

[27] D.R. Harries and G.H. Broomfield, J. Nucl. Mater. 9 (1963) 327.

[28] T. Kato, K. Nakata, J. Kuniya, S. Oknuki and H. Taka-

hashi, J. Nucl. Mater. 155-157 (1988) 856.

[29] C.L. Briant, Metallurgical aspect of environmental fail- ures, Materials Science Monographs, vol. 12 (Elsevier,

1985) p. 132.

[30] R.C. Newman and A. Merka, Proc. Environment-In- duced cracking of metals, NACE-10, Kohler, Wisconsin,

2-7 October 1988, eds. R.P. Gangloff and M.B. Ives,

(NACE, Houston, 1990) p. 489.

[31] T. Angel, J. Iron Steel Inst. 177 (1954) 165.

[32] B.C. Odegard, J.A. Brooks and A.J. West, Proc. Effect of Hydrogen on Behaviour of Materials, Moran, Wyoming,

7-11 September 1975 (AIME, Warrendale, Pennsylvania,

19761 p. 116.

[33] D. Eliezer, Proc. Hydrogen effects in metals, Moran,

Wyoming, August 26-31, 1980 (AIME, Warrendale, Pennsylvania 1981) p. 565.

[34] A.J. West and J.A. Brooks, Proc. Effect of hydrogen on

behaviour of materials, Moran, Wyoming, 7-11 Septem-

ber 1975 (AIME, Warrendale, Pennsylvania, 1976) p.

686.

[35] R.L. Kesterson, ASTM STP 543 Hydrogen Embrittle-

ment Testing, Los Angeles, 25-30 June 1972 (ASTM, 1974) p. 254.

[36] D.R. Harries, J. Nucl. Mater. 82 (1979) 2.

[37] N. Kishimoto, R.E. Clausing, L. Heatherly Jr. and K.

Farrel, J. Nucl. Mater. 179-181 (1991) 998. 1381 H.T. Him and B.A. Chin, J. Nucl. Mater. 179-181 (1991)

1131.

[39] P.J. Maziasz, Perspective on present and future alloy

development efforts on austenitic stainless steels for fu-

sion application, Proc. Int. Conf. on Fusion Reactor

Materials, Tokyo, 3-12 December 1984; Report 9514868,

Oak Ridge National Laboratory (1984).

[40] R.E. Clausing and E.E. Bloom, Proc. 4th Bolton Landing

Conf. on Grain boundaries in Engineering Materials,

Lake George, 9-12 June 1974 (1975) p. 491.

[41] M. Kangilaski, J.W. Spretnak, A.A. Bauer and R.A.

Wullaert, Proc. irradiation effects on structural alloys for

nuclear reactor applications, Toronto, 29 June-l July,

1970, ASTM-STP 484 (1970) p. 194.

[42] A.W. Thompson, Mater. Sci. Eng. 21 (1975) 41.

[43] A.J. West and D.E. Rawl, Proc. Conf. on Hydrogen in

Stainless Steels: Isotopic Effects on Mechanical Proper-

ties, Dayton, 29 April-l May 1980 CANS, La Grange

Park, IL, 19801 p. 69.

[44] A.J. Jacobs, R.E. Clausing, M.K. Miller and C.M. Shep-

herd, Proc. 4th Int. Symp. on Environmental Degrada-

tion of Materials in Nuclear Power Systems - Water

Reactors, 6-10 August 1989, Jekyll Island, Georgia

(NACE, Houston, 1990) p. 14.21.

[45] C.M. Shepherd and T.M. Williams, Proc. 4th Int. Symp.

on Environmental Degradation of Materials in Nuclear

Power Systems - Water Reactors, 6-10 August 1989,

Jekyll Island, Georgia (NACE, Houston, 1990) p. 14.11.

[46] A.J. Jacobs, C.M. Shephard, G.E.C. Bell and G.P.

Wozadlo, Proc. 5th Int. Symp. on Environmental Degra-

dation of Materials in Nuclear Power Systems - Water

Reactors, 25-29 August 1991, Monterey, CA CANS, La

Grange Park, IL, 1992) p. 917.

[47] K. Asano, K. Fuhuya, K. Nakata and M. Kodama, Proc.

5th Int. Symp. on Environmental Degradation of Materi-

als in Nuclear Power Systems - Water Reactors, 25-29

August 1991, Monterey, CA CANS, La Grange Park, IL,

1992) p. 838.

[48] S.M. Bruemmer, E.P. Simonen and L.A. Charlot, Proc.

4th Int. Symp. on Environmental Degradation of Materi-

als in Nuclear Power Systems - Water Reactors, 6-10

August 1989, Jekyll Island, Georgia (NACE, Houston,

1990) p. 14.1.

1491 D.I.R. Norris, C. Baker and J.M. Titchmarsch, Proc.

Conf. on Radiation-Induced Sensitization of Stainless

Steels, CEGB Berkeley, Nuclear Laboratory, September 1986 (CEGB, 1986) p. 86.

[50] E.P. Simonen and R.H. Jones, Proc. 3rd Int. Symp. on

Environmental Degradation of Materials in Nuclear

Power Systems - Water Reactors, Traverse City, 30

August-3 September 1987 (AIME, Warrendale, Pennsyl-

vania, 1988) p. 683.

[51] H.M. Chung, W.E. Ruther, J.E. Sanecki and T.F. Kass-

ner, Proc. 5th Int. Symp. on Environmental Degradation

of Materials in Nuclear Power Systems - Water Reac-

tors, 25-29 August 1991, Monterey, CA CANS, La Grange

Park, IL, 1992) p. 795.

1521 Detecting susceptibility to intergranular attack in

austenitic stainless steels, Practices E and F, ASTM Standard A262-86, vol. 03.02 (1990).

1531 W.L. Clarke, R.L. Cowan and W.L. Walker, Comparative

methods for measuring degree of sensitization on stain- less steels, ASTM-STP 656 (1978) p. 99.

Page 22: A review of irradiation assisted stress corrosion …...ELSEVIER Journal of Nuclear Materials 211(1994) 101-122 Review article A review of irradiation assisted stress corrosion cracking

122 P. Scott/Journal of Nuclear Materials 211 (1994) 101-122

[54] T. Inazumi, G.E.C. Bell, E.A. Kenik and K. Kiuchi, Corrosion 46 (1990) 786.

[55] Detecting susceptibility to intergranular attack in

austenitic stainless steels, Practices C and D, ASTM

Standard A262-86, vol. 03.02 (19901.

[56] A.J. Jacobs, Corrosion 46 (1990) 634.

[57] A.J. Jacobs, Corrosion 46 (1990) 30.

[58] M. Kodama, S. Mishimura, J. Morisaura, S. Suzuki, S.

Shina and M. Yamamoto, Proc. 5th Int. Symp. on Envi-

ronmental Degradation of Materials in Nuclear Power

Systems - Water Reactors, 25-29 August 1991, Mon-

terey, CA CANS, La Grange Park, IL, 19921 p. 948.

[59] S. Bruemmer, L.A. Charlot and E.P. Simonen, Proc. 5th

Int. Symp. on Environmental Degradation of Materials in

Nuclear Power Systems - Water Reactors, 25-29 August

1991, Monterey, CA CANS, La Grange Park, IL, 1992) p.

821.

[60] A.J. Jacobs, G.P. Wozadlo and S.A. Wilson, Corrosion 49

(1993) 145.

[61] F. Garzarolli, D. Alter, P. Dewers and J.L. Nelson, Proc.

3rd Int. Symp. on Environmental Degradation of Materi-

als in Nuclear Power Systems - Water Reactors, Tra-

verse City, Michigan, 30 August-3 September 1987

(AIME, Warrendale, Pennsylvania, 19881 p. 657.

[62] K. Fukuya, N. Nakata and A. Horie, Proc. 5th Int. Symp.

on Environmental Degradation of Materials in Nuclear

Power Systems - Water Reactors, 25-29 August 1991,

Monterey, CA, CANS, La Grange Park, IL, 1992) p. 814.

[63] F. Garzarolli, P. Dewes, R. Hahn and J.L. Nelson, De-

formability of high purity stainless steels and Ni based

alloys in the core of a PWR, Proc. 6th Int. Symp. on

Environmental Degradation of Materials in Nuclear

Power Systems - Water Reactors, San Diego, CA, Au-

gust 1-5, 1993, to be published.

[64] P.J. Sipush, J. Woodcock and R.W. Chickering, Lifetime

of PWR Silver-Indium-Cadmium Control rods, EPRI

Report NP 4512 (1986).